Physical Properties | Metric | English | Comments |
---|
Density | 7.80 g/cc | 0.282 lb/in³ |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Brinell | 180 @Thickness >=25.0 mm | 180 @Thickness >=0.984 in |
| 185 @Thickness 15.0 - 25.0 mm | 185 @Thickness 0.591 - 0.984 in |
| 190 @Thickness <=15.0 mm | 190 @Thickness <=0.591 in |
| 200 @Thickness 24.0 - 190 mm | 200 @Thickness 0.945 - 7.48 in |
| 200 @Thickness 24.0 - 190 mm | 200 @Thickness 0.945 - 7.48 in |
Tensile Strength | 550 MPa @Thickness 24.0 - 190 mm | 79800 psi @Thickness 0.945 - 7.48 in |
| 550 MPa @Thickness 24.0 - 190 mm | 79800 psi @Thickness 0.945 - 7.48 in |
| 560 MPa @Thickness >=25.0 mm | 81200 psi @Thickness >=0.984 in |
| 580 MPa @Thickness 15.0 - 25.0 mm | 84100 psi @Thickness 0.591 - 0.984 in |
| 600 MPa @Thickness <=15.0 mm | 87000 psi @Thickness <=0.591 in |
Tensile Strength, Yield | >= 380 MPa @Thickness >=25.0 mm | >= 55100 psi @Thickness >=0.984 in |
| >= 400 MPa @Thickness 15.0 - 25.0 mm | >= 58000 psi @Thickness 0.591 - 0.984 in |
| >= 410 MPa @Thickness 24.0 - 190 mm | >= 59500 psi @Thickness 0.945 - 7.48 in |
| >= 410 MPa @Thickness 24.0 - 190 mm | >= 59500 psi @Thickness 0.945 - 7.48 in |
| >= 430 MPa @Thickness <=15.0 mm | >= 62400 psi @Thickness <=0.591 in |
Elongation at Break | 19 % @Thickness 24.0 - 190 mm | 19 % @Thickness 0.945 - 7.48 in |
| 19 % @Thickness 24.0 - 190 mm | 19 % @Thickness 0.945 - 7.48 in |
| 25 % @Thickness <=15.0 mm | 25 % @Thickness <=0.591 in |
| 25 % @Thickness 15.0 - 25.0 mm | 25 % @Thickness 0.591 - 0.984 in |
| 25 % @Thickness >=25.0 mm | 25 % @Thickness >=0.984 in |
Modulus of Elasticity | 210 GPa | 30500 ksi |
Poissons Ratio | 0.30 | 0.30 |
Shear Modulus | 80.0 GPa | 11600 ksi |
Impact Test | 27.0 J @Thickness 24.0 - 190 mm, Temperature 20.0 °C | 19.9 ft-lb @Thickness 0.945 - 7.48 in, Temperature 68.0 °F |
| 27.0 J @Thickness 24.0 - 190 mm, Temperature -40.0 °C | 19.9 ft-lb @Thickness 0.945 - 7.48 in, Temperature -40.0 °F |
| 27.0 J @Thickness <=15.0 mm, Temperature -40.0 °C | 19.9 ft-lb @Thickness <=0.591 in, Temperature -40.0 °F |
| 27.0 J @Thickness 15.0 - 25.0 mm, Temperature -40.0 °C | 19.9 ft-lb @Thickness 0.591 - 0.984 in, Temperature -40.0 °F |
| 27.0 J @Thickness >=25.0 mm, Temperature -40.0 °C | 19.9 ft-lb @Thickness >=0.984 in, Temperature -40.0 °F |
|
Electrical Properties | Metric | English | Comments |
---|
Electrical Resistivity | 0.00000200 - 0.00000250 ohm-cm | 0.00000200 - 0.00000250 ohm-cm |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear | 12.0 µm/m-°C @Temperature 20.0 - 300 °C | 6.67 µin/in-°F @Temperature 68.0 - 572 °F |
Specific Heat Capacity | 0.460 - 0.480 J/g-°C @Temperature 50.0 - 100 °C | 0.110 - 0.115 BTU/lb-°F @Temperature 122 - 212 °F |
Thermal Conductivity | 40.0 - 45.0 W/m-K | 278 - 312 BTU-in/hr-ft²-°F |
Transformation Temperature | 395 °C | 743 °F |
| 721 °C | 1330 °F |
| 810 °C | 1490 °F |
|
Component Elements Properties | Metric | English | Comments |
---|
Carbon, C | 0.17 - 0.20 % | 0.17 - 0.20 % |
Chromium, Cr | 0.20 - 0.28 % | 0.20 - 0.28 % |
Iron, Fe | 96.99 - 97.78 % | 96.99 - 97.78 % |
Manganese, Mn | 1.45 - 1.6 % | 1.45 - 1.6 % |
Molybdenum, Mo | <= 0.10 % | <= 0.10 % |
Nickel, Ni | <= 0.20 % | <= 0.20 % |
Phosphorus, P | <= 0.025 % | <= 0.025 % |
Silicon, Si | 0.30 - 0.45 % | 0.30 - 0.45 % |
Sulfur, S | 0.020 - 0.035 % | 0.020 - 0.035 % |
Vanadium, V | 0.080 - 0.12 % | 0.080 - 0.12 % |
|
Descriptive Properties |
---|
Dl | 1.6-1.9% |
Weldability | CEV 0.6max |
| Pcm 0.35max |
Some of the values displayed above may have been converted from their original units and/or rounded in order to
display the information in a consistent format. Users requiring more precise data for scientific or engineering
calculations can click on the property value to see the original value as well as raw conversions to equivalent units.
We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding
error. We also ask that you refer to MatWeb's
terms of use regarding this information.
Click here to view
all the property values for this datasheet as they were originally entered into MatWeb.