MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

USP Class VI Adhesives
USP Class VI Approved Adhesives for Medical Device Applications
Master Bond’s biocompatible adhesives are designed to meet the needs of medical device manufacturers. Compounds withstand various types of sterilization methods.

Eastman Tritan™ MX731 Medical Grade Copolyester
Categories: Polymer; Thermoplastic; Polyester, TP

Material Notes: Eastman Tritan Copolyester MX731 is an amorphous product with excellent appearance and clarity. Eastman Tritan Copolyester MX731 is a high flow medical grade of Eastman Tritan that has viscosity reductions of 40-50% relative to Eastman Tritan Copolyester MX711. Eastman Tritan Copolyester MX731contains a mold release derives from vegetable based sources. Eastman Tritan Copolyester MX731 has many outstanding features that include excellent toughness, hydrolytic stability, heat resistance, chemical resistance, and melt flowability. Eastman Tritan Copolyester MX731 has been formulated for medical devices. Eastman Tritan Copolyester MX731 has been tested for FDA/ISO 10993 and USP Class VI Biological Evaluation testing after Gamma and ETO sterilization.

Application/Uses

  • Blood therapy
  • IV components

Key Attributes

  • Ease of processing
  • Excellent clarity
  • Excellent hydrolytic stability
  • Fast cycle times
  • Fast drying times
  • Good chemical resistance
  • Good color stability upon ETO sterilization
  • Good color stability upon gamma sterilization
  • Good heat resistance
  • Good melt flowability
  • Good toughness

Information was provided by Eastman.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.18 g/cc1.18 g/ccASTM D792
Linear Mold Shrinkage 0.0050 - 0.0070 cm/cm0.0050 - 0.0070 in/inASTM D955
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 111111ASTM D785
Tensile Strength at Break 52.0 MPa7540 psiASTM D638
Tensile Strength, Yield 43.0 MPa6240 psiASTM D638
Elongation at Break 210 %210 %ASTM D638
Elongation at Yield 7.0 %7.0 %ASTM D638
Tensile Modulus 1.575 GPa228.4 ksiASTM D638
Flexural Yield Strength 64.0 MPa9280 psiASTM D790
Flexural Modulus 1.575 GPa228.4 ksiASTM D790
Izod Impact, Notched 8.60 J/cm16.1 ft-lb/inASTM D256
Izod Impact, Unnotched NBNBASTM D4812
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 0.46 MPa (66 psi) 94.0 °C201 °FASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 81.0 °C178 °FASTM D648
 
Optical PropertiesMetricEnglishComments
Haze <= 1.0 %<= 1.0 %ASTM D1003
Transmission, Visible 91 %91 %ASTM D1003
 
Processing PropertiesMetricEnglishComments
Processing Temperature 260 - 282 °C500 - 540 °F
Mold Temperature 38.0 - 66.0 °C100 - 151 °F
Drying Temperature 88.0 °C190 °F
Dry Time 4 - 6 hour4 - 6 hour
 
Compliance PropertiesMetricEnglishComments
USP Class VI YesYes

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Eastman Tritan™ MX711 Medical Grade Copolyester
Eastman Tritan™ MX730 Medical Grade Copolyester
Eastman Tritan™ MP100 Copolyester
Eastman Tritan™ MX710 Medical Grade Copolyester
Eastman Tritan™ TX2000 Copolyester

PE8917 / 109259

USP Class VI Adhesives
USP Class VI Approved Adhesives for Medical Device Applications
Master Bond’s biocompatible adhesives are designed to meet the needs of medical device manufacturers. Compounds withstand various types of sterilization methods.

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.