MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Nylon

(Viewing data as-entered. Click here to return)
Nylacast Nylube Cast Nylon 6, Lubricated (Blended Solid and Liquid Lubricant)
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6)

Material Notes: Nylube was introduced into the Nylacast product range in 1989 as a logical progression to Oilon with already outstanding performance as a bearing material. Since that time, it has proved to be Nylacast’s supreme wear resisting grade and one of the most important developments from Nylacast in new materials. Nylube contains a combined liquid/solid lubricant system which allows for a coefficient of friction as low as 0.08. This is below that of almost any other polymer available at present. Nylube has substantially improved the wear resistance abilities compared to that of any other currently available lubricated grade of cast nylon, whilst retaining excellent physical property characteristics. The material is particularly suited to dry running bearing applications throughout a wide load, speed and temperature range (up to 120ºC). Like Oilon, Nylube is suitable for use in applications in the food and pharmaceutical industries.

Benefits:

  • Outstanding wear and abrasion resistance
  • Significantly improved PV characteristics
  • Improved operating temperature capability
  • Outstanding lubrication and low coefficient of friction
  • Greatly improved stick/slip capabilities
  • Wide load, speed and temperature operating range
  • Consistent wear performance throughout product life
  • Excellent dimensional stability
  • Reduced water absorption
  • Excellent chemical resistance
  • Blended solid/liquid lubricant system
  • FDA compliant for direct food contact applications
Typical Application:
  • Wear pads
  • Stabilisers
  • Stoppers
  • Pulleys
  • L-shape wear pads
  • Sheaves
  • Rollers
  • Sliders
  • Stoppers
  • Bushes
  • Slide pads
  • Bearings
  • Gears
  • Winches
  • Bespoke Components

Information provided by Nylacast Ltd.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 1.14 g/ccmethod A; ISO 1183:1987
Water Absorption 0.20 %
@Time 86400 sec
Immersion @ 23°C; ISO 62:1999
Moisture Absorption at Equilibrium 2.0 %50% RH, 23°C; ISO 62:1999
Water Absorption at Saturation 5.9 %
@Time 86400 sec
Immersion @ 23°C; ISO 62:1999
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 83ISO 868:2003
Tensile Strength, Yield 89.0 - 90.0 MPaSample Type 1B, 50mm/min; ISO 527-1/2:1993
Elongation at Break >= 30 %Type 1B, 50mm/min; ISO 527-1/2:1993
Tensile Modulus 3600 - 4000 MPaE-modulus; Type 1B, 50mm/min; ISO 527-1/2:1993
Flexural Strength 115 - 125 MPa1.5mm/min; ISO 178:2001
Flexural Modulus 3350 - 3600 MPa1.5mm/min; ISO 178:2001
Compressive Strength 105 - 125 MPaType B, 5mm/min; ISO 604:2002
Compressive Modulus 2500 - 2700 MPaType B, 5mm/min; ISO 604:2002
Izod Impact, Notched (ISO) 5.50 - 7.00 kJ/m²Type A; ISO 180:2000
Coefficient of Friction, Dynamic 0.075
@Pressure 1.75 MPa
31.4m/min
K Factor (Wear Factor) 3.90e+6
@Pressure 1.75 MPa
[m*3/Nm], 31.4m/min
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity >= 1.00e+15 ohm-cmIEC 60093:1980-01
Surface Resistance >= 1.00e+14 ohmIEC 60093:1980-01
Dielectric Constant 3.7
@Frequency 1e+6 Hz
IEC 60250:1969-01
 4.0
@Frequency 100 Hz
IEC 60250:1969-01
Dielectric Strength 25.0 kV/mmIEC 60243-1:1998-01
Dissipation Factor 0.013
@Frequency 100 Hz
IEC 60250:1969-01
Comparative Tracking Index 600 VIEC 60112:2003-01
 
Thermal PropertiesOriginal ValueComments
CTE, linear 80.0 µm/m-°C
@Temperature 23.0 - 55.0 °C
ISO 11359-2:1999
Thermal Conductivity 0.250 W/m-KMean T = 20°C; ISO 8301:1991
Melting Point 222 °C
Maximum Service Temperature, Air 180 °CIntermittent
 110 °C
@Time 1.80e+7 sec
Continuous
Deflection Temperature at 1.8 MPa (264 psi) 75.0 °CISO 75
Minimum Service Temperature, Air -100 °CIntermittent
 -40.0 °CContinuous
Glass Transition Temp, Tg 65.0 °CISO 11359:1999
Flammability, UL94 HBIEC 60695-11-10:2003-08
 
Compliance PropertiesOriginal ValueComments
FDA Yes
 
Descriptive Properties
ColorRed, Black, Natural
Limiting PV100 MPa/m

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Nylacast Oilon Cast Nylon 6, Lubricated (Lubricant Oil Filled)
Nylacast Nylube MO Cast Nylon 6, Lubricated (Blended Solid and Liquid Lubricant), MoS2 Filled
Overview of materials for Nylon 6, MoS2 Filled
Okulen® 2000 PE-UHMW, DryRun
Nylacast Nylube GF Cast Nylon 6, Lubricated (Blended Solid and Liquid Lubricant), Glass Filled

PNYLAC07 / 89265

Nylon

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.