MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
3M Fastbond™ 2000-NF Contact Adhesive with Spray Activator #1
Categories: Polymer; Adhesive

Material Notes: 3M Fastbond™ Contact Adhesive 2000-NF with Spray Activator #1 is a water-dispersed, high solid, activated adhesive which provides immediate bonding capabilities and handling strength without forced drying equipment for most applications.

Information provided by 3M

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Solids Content 15 - 19 %Spray Activator #1
 47 - 51 %2000-NF
Viscosity 250 - 750 cP
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 0.172 MPa
@Temperature 82.0 °C
Flatwise, aged 3 weeks at 24°C/50% RH, separation rate of 0.05 in/min; ASTM C297
 0.172 MPa
@Temperature 93.0 °C
Flatwise, aged 3 weeks at 24°C/50% RH, separation rate of 0.05 in/min; ASTM C297
 0.172 MPa
@Temperature 107 °C
Flatwise, aged 3 weeks at 24°C/50% RH, separation rate of 0.05 in/min; ASTM C297
 0.579 MPa
@Temperature 24.0 °C
Flatwise, aged 3 weeks at 24°C/50% RH, separation rate of 0.05 in/min; ASTM C297
Shear Strength 30.0 psi
@Temperature 107 °C
Overlap, 1/8 birch to 1/8 birch, bond tested after aging 3 weeks @ 24°C and 50% RH at a separation rate of 0.2 in/min; ASTM D1002
 40.0 psi
@Temperature 93.0 °C
Overlap, 1/8 birch to 1/8 birch, bond tested after aging 3 weeks @ 24°C and 50% RH at a separation rate of 0.2 in/min; ASTM D1002
 50.0 psi
@Temperature 82.0 °C
Overlap, 1/8 birch to 1/8 birch, bond tested after aging 3 weeks @ 24°C and 50% RH at a separation rate of 0.2 in/min; ASTM D1002
 350 psi
@Temperature 24.0 °C
Overlap, 1/8 birch to 1/8 birch, bond tested after aging 3 weeks @ 24°C and 50% RH at a separation rate of 0.2 in/min; ASTM D1002
 1000 psi
@Temperature -37.0 °C
Overlap, 1/8 birch to 1/8 birch, bond tested after aging 3 weeks @ 24°C and 50% RH at a separation rate of 0.2 in/min; ASTM D1002
 55.0 psi
@Time Error in fixSigDigits: @digits must be between 1 a sec
Overlap of Build-Up, 1/8 birch to 1/8 birch, 25°C at 50% RH Aged; ASTM D1002
 55.0 psi
@Time Error in fixSigDigits: @digits must be between 1 a sec
Overlap of Build-Up, 1/8 birch to 1/8 birch, 32°C at 90% RH Aged; ASTM D1002
 75.0 psi
@Time 900 sec
Overlap of Build-Up, 1/8 birch to 1/8 birch, 25°C at 50% RH Aged; ASTM D1002
 75.0 psi
@Time 900 sec
Overlap of Build-Up, 1/8 birch to 1/8 birch, 32°C at 90% RH Aged; ASTM D1002
 130 psi
@Time 1800 sec
Overlap of Build-Up, 1/8 birch to 1/8 birch, 25°C at 50% RH Aged; ASTM D1002
 160 psi
@Time 1800 sec
Overlap of Build-Up, 1/8 birch to 1/8 birch, 32°C at 90% RH Aged; ASTM D1002
 160 psi
@Time 3600 sec
Overlap of Build-Up, 1/8 birch to 1/8 birch, 25°C at 50% RH Aged; ASTM D1002
 165 psi
@Time 5400 sec
Overlap of Build-Up, 1/8 birch to 1/8 birch, 25°C at 50% RH Aged; ASTM D1002
 170 psi
@Time 7200 sec
Overlap of Build-Up, 1/8 birch to 1/8 birch, 25°C at 50% RH Aged; ASTM D1002
 180 psi
@Time 3600 sec
Overlap of Build-Up, 1/8 birch to 1/8 birch, 32°C at 90% RH Aged; ASTM D1002
 190 psi
@Time 5400 sec
Overlap of Build-Up, 1/8 birch to 1/8 birch, 32°C at 90% RH Aged; ASTM D1002
 190 psi
@Time 7200 sec
Overlap of Build-Up, 1/8 birch to 1/8 birch, 32°C at 90% RH Aged; ASTM D1002
 215 psi
@Time 14400 sec
Overlap of Build-Up, 1/8 birch to 1/8 birch, 32°C at 90% RH Aged; ASTM D1002
 230 psi
@Time 14400 sec
Overlap of Build-Up, 1/8 birch to 1/8 birch, 25°C at 50% RH Aged; ASTM D1002
 255 psi
@Time 28800 sec
Overlap of Build-Up, 1/8 birch to 1/8 birch, 32°C at 90% RH Aged; ASTM D1002
 260 psi
@Time 28800 sec
Overlap of Build-Up, 1/8 birch to 1/8 birch, 25°C at 50% RH Aged; ASTM D1002
 290 psi
@Time 86400 sec
Overlap of Build-Up, 1/8 birch to 1/8 birch, 25°C at 50% RH Aged; ASTM D1002
 315 psi
@Time 86400 sec
Overlap of Build-Up, 1/8 birch to 1/8 birch, 32°C at 90% RH Aged; ASTM D1002
 320 psi
@Time 259000 sec
Overlap of Build-Up, 1/8 birch to 1/8 birch, 25°C at 50% RH Aged; ASTM D1002
 340 psi
@Time 259000 sec
Overlap of Build-Up, 1/8 birch to 1/8 birch, 32°C at 90% RH Aged; ASTM D1002
 350 psi
@Time 605000 sec
Overlap of Build-Up, 1/8 birch to 1/8 birch, 25°C at 50% RH Aged; ASTM D1002
 350 psi
@Time 605000 sec
Overlap of Build-Up, 1/8 birch to 1/8 birch, 32°C at 90% RH Aged; ASTM D1002
 350 psi
@Time 1.21e+6 sec
Overlap of Build-Up, 1/8 birch to 1/8 birch, 25°C at 50% RH Aged; ASTM D1002
 350 psi
@Time 1.21e+6 sec
Overlap of Build-Up, 1/8 birch to 1/8 birch, 32°C at 90% RH Aged; ASTM D1002
 350 psi
@Time 1.81e+6 sec
Overlap of Build-Up, 1/8 birch to 1/8 birch, 25°C at 50% RH Aged; ASTM D1002
 350 psi
@Time 1.81e+6 sec
Overlap of Build-Up, 1/8 birch to 1/8 birch, 32°C at 90% RH Aged; ASTM D1002
 
Descriptive Properties
AppearanceBlue, Light Orange or Neutral2000-NF
 ClearSpray Activator #1
BaseInorganic SaltSpray Activator #1
 Polychloroprene2000-NF

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PMM34039 / 168786

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.