Physical Properties | Original Value | Comments |
---|
Specific Gravity | 0.950 g/cc |
|
Mechanical Properties | Original Value | Comments |
---|
Hardness, Shore D | 40 |
| 40 |
| 40 |
| 40 |
| 41 |
| 41 |
| 41 |
| 42 |
| 42 |
| 44 |
| 45 |
| 46 |
| 47 |
| 50 |
| 50 |
| 40 @Time 5.00 sec |
Tensile Strength | 2690 psi |
| 2750 psi |
| 1650 psi @Treatment Temp. 150 °C, Time 3.60e+6 sec |
| 2020 psi @Treatment Temp. 150 °C, Time 2.59e+6 sec |
| 2540 psi @Treatment Temp. 150 °C, Time 605000 sec |
| 2560 psi @Treatment Temp. 100 °C, Time 3.60e+6 sec |
| 2580 psi @Treatment Temp. 150 °C, Time 1.30e+6 sec |
| 2590 psi @Treatment Temp. 100 °C, Time 605000 sec |
| 2640 psi @Treatment Temp. 150 °C, Time 86400 sec |
| 2650 psi @Treatment Temp. 125 °C, Time 1.30e+6 sec |
| 2650 psi @Treatment Temp. 100 °C, Time 2.59e+6 sec |
| 2660 psi @Treatment Temp. 100 °C, Time 86400 sec |
| 2730 psi @Treatment Temp. 125 °C, Time 605000 sec |
| 2760 psi @Treatment Temp. 125 °C, Time 86400 sec |
| 2790 psi @Treatment Temp. 125 °C, Time 3.60e+6 sec |
| 2830 psi @Treatment Temp. 100 °C, Time 1.30e+6 sec |
| 2830 psi @Treatment Temp. 125 °C, Time 2.59e+6 sec |
Elongation at Break | 530 % |
| 10 % @Treatment Temp. 150 °C, Time 3.60e+6 sec |
| 180 % @Treatment Temp. 150 °C, Time 2.59e+6 sec |
| 390 % @Treatment Temp. 150 °C, Time 605000 sec |
| 390 % @Treatment Temp. 150 °C, Time 1.30e+6 sec |
| 450 % @Treatment Temp. 150 °C, Time 86400 sec |
| 470 % @Treatment Temp. 125 °C, Time 3.60e+6 sec |
| 490 % @Treatment Temp. 125 °C, Time 1.30e+6 sec |
| 500 % @Treatment Temp. 125 °C, Time 2.59e+6 sec |
| 510 % @Treatment Temp. 100 °C, Time 3.60e+6 sec |
| 520 % @Treatment Temp. 100 °C, Time 86400 sec |
| 530 % @Treatment Temp. 100 °C, Time 1.30e+6 sec |
| 530 % @Treatment Temp. 100 °C, Time 2.59e+6 sec |
| 530 % @Treatment Temp. 125 °C, Time 86400 sec |
| 530 % @Treatment Temp. 125 °C, Time 605000 sec |
| 540 % @Treatment Temp. 100 °C, Time 605000 sec |
Elongation, Ultimate | 600 % |
Tensile Modulus | 5.70 MPa @Temperature 125 °C |
| 12.5 MPa @Temperature 100 °C |
| 125 MPa @Temperature 23.0 °C |
100% Modulus | 1250 psi |
| 1330 psi |
| 1410 psi @Treatment Temp. 100 °C, Time 86400 sec |
| 1410 psi @Treatment Temp. 100 °C, Time 605000 sec |
| 1450 psi @Treatment Temp. 125 °C, Time 86400 sec |
| 1460 psi @Treatment Temp. 100 °C, Time 1.30e+6 sec |
| 1470 psi @Treatment Temp. 100 °C, Time 2.59e+6 sec |
| 1480 psi @Treatment Temp. 100 °C, Time 3.60e+6 sec |
| 1490 psi @Treatment Temp. 125 °C, Time 605000 sec |
| 1520 psi @Treatment Temp. 150 °C, Time 86400 sec |
| 1580 psi @Treatment Temp. 150 °C, Time 605000 sec |
| 1580 psi @Treatment Temp. 125 °C, Time 1.30e+6 sec |
| 1580 psi @Treatment Temp. 125 °C, Time 2.59e+6 sec |
| 1640 psi @Treatment Temp. 125 °C, Time 3.60e+6 sec |
| 1720 psi @Treatment Temp. 150 °C, Time 1.30e+6 sec |
| 1840 psi @Treatment Temp. 150 °C, Time 2.59e+6 sec |
Flexural Modulus | 140 MPa |
Tear Strength | 203 pli @Temperature 100 °C |
| 369 pli @Temperature 25.0 °C |
Compression Set | 39 % @Treatment Temp. 25.0 °C, Time 79200 sec |
| 65 % @Treatment Temp. 100 °C, Time 79200 sec |
Tensile Set | 48.0 % |
|
Thermal Properties | Original Value | Comments |
---|
Brittleness Temperature | -71.0 °F |
Shrinkage | 24 % |
| 24 % |
| 24 % |
| 168 % |
| 168 % |
| 168 % |
| 360 % |
| 360 % |
| 360 % |
| 720 % |
| 720 % |
| 720 % |
| 1000 % |
| 1000 % |
| 1000 % |
Some of the values displayed above may have been converted from their original units and/or rounded in order to
display the information in a consistent format. Users requiring more precise data for scientific or engineering
calculations can click on the property value to see the original value as well as raw conversions to equivalent units.
We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding
error. We also ask that you refer to MatWeb's
terms of use regarding this information.
Click here to go back to viewing the property data in MatWeb's normal format.