MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Chemours Viton® A-361C with 60 MT Black Fluoroelastomer Compound
Categories: Polymer; Thermoset; Fluoropolymer, TS; Thermoset Fluoroelastomer; Rubber or Thermoset Elastomer (TSE)

Material Notes:
  • Intermediate viscosity level (when compared with Viton® A-201C/Viton® A-401C)
  • Fully precompounded with reduced curative level and Incorporated metal adhesion promoter
  • Improved processing with increased mold flow, easier mold release with less mold fouling, and improved demolding “hot tear”
  • Good metal bonding with standard industrial primers

Applications

  • Compression, transfer, and injection molding of: O-rings and gaskets, Valve stem and crankshaft seals (and other bonded parts requiring fluid and heat resistance of the A-family of Viton®)

    Chemours was formed from former DuPont performance chemicals businesses, including the Viton product line, in 2015.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Mooney Viscosity 97
@Temperature 121 °C
ML (1+10), Uncompounded Viton; ASTM D1646
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 90No Postcure; ASTM D2240
 9024 hours Postcure; ASTM D2240
Tensile Strength at Break 9.60 MPaNo Postcure; ASTM D412
 14.4 MPa24 hours Postcure; ASTM D412
Elongation at Break 152 %24 hours Postcure; ASTM D412
 226 %No Postcure; ASTM D412
100% Modulus 0.00640 GPa
@Strain 100 %
No Postcure; ASTM D412
 0.0103 GPa
@Strain 100 %
24 hours Postcure; ASTM D412
Compression Set 16 %
@Temperature 23.0 °C,
Time 252000 sec
O-Rings; ASTM D395B
 24 %
@Temperature 200 °C,
Time 252000 sec
O-Rings; ASTM D395B
 47 %
@Temperature 232 °C,
Time 252000 sec
O-Rings; ASTM D395B
 
Processing PropertiesOriginal ValueComments
Processing Temperature 177 °C
@Time 601 sec
Slab Cure
 232 °C
@Time 86400 sec
Postcure
 
Descriptive Properties
Formulation as Tested100A361C
 3MgO
 6Ca(OH)2
 60MT Black

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
AlphaGary PVC 2235RSM-100 CLEAR 000X Polyvinyl Chloride Thermoplastic
Precision Polymer Engineering E90Q Ethylene Propylene Rubber
AlphaGary PVC 2212-100 CLEAR 0003 Polyvinyl Chloride Thermoplastic
Ellay Ellay™ 0-4113 Plasticized Polyvinyl Chloride Biomedical Elastomer
Chemours Viton® A-700 with 65 phr N990 Carbon Black

PDVC9901 / 170542

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.