MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Celanese Hytrel® 5555HS TPC-ET
Categories: Polymer; Thermoplastic; Elastomer, TPE; Polyester TPE

Material Notes: 55 Shore D High Performance Polyester Elastomer with Heat Ageing Protection

Former DuPont product acquired by Celanese in 2022.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.19 g/ccISO 1183
Water Absorption 0.70 %
@Time 86400 sec
Immersion; Sim. to ISO 62
 0.60 %
@Thickness 2.00 mm
Sim. to ISO 62
Moisture Absorption 0.200 %
@Thickness 2.00 mm
Sim. to ISO 62
Linear Mold Shrinkage, Flow 0.013 cm/cmISO 294-4, 2577
Linear Mold Shrinkage, Transverse 0.014 cm/cmISO 294-4, 2577
Melt Flow 8.5 g/10 min
@Load 2.16 kg,
Temperature 220 °C
cm³/10min Volumetric; ISO 1133
 8.5 g/10 min
@Load 2.16 kg,
Temperature 220 °C
ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 5215s; ISO 48-4
 <= 55ISO 48-4
Tensile Stress at Strain 6.90 MPa
@Strain 5.0 %
1BA specimen at 50mm/min; ISO 527-1/-2
 11.1 MPa
@Strain 10 %
ISO 527-1/-2
 14.7 MPa
@Strain 50 %
ISO 527-1/-2
 16.0 MPa
@Strain 100 %
ISO 527-1/-2
Tensile Modulus 190 MPaISO 527-1/-2
Flexural Modulus 195 MPaISO 178
Poissons Ratio 0.48
Charpy Impact Unnotched NB
@Temperature 23.0 °C
ISO 179/1eU
Tensile Impact Strength 300 kJ/m²
@Temperature 23.0 °C
Notched; ISO 8256/1
Tensile Creep Modulus, 1 hour 140 MPa1h; ISO 899-1
Tensile Creep Modulus, 1000 hours 100 MPa1000h; ISO 899-1
Tear Strength 166 kN/mnormal; ISO 34-1
 172 kN/mparallel; ISO 34-1
Abrasion 120mm3; ISO 4649
Compression Set 60 %
@Temperature 70.0 °C,
Time 86400 sec
ISO 815
 
Electrical PropertiesOriginal ValueComments
Comparative Tracking Index 600 VIEC 60112
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 180 µm/m-°CISO 11359-1/-2
CTE, linear, Transverse to Flow 180 µm/m-°CISO 11359-1/-2
Melting Point 201 °C10°C/min; ISO 11357-1/-3
Deflection Temperature at 0.46 MPa (66 psi) 78.0 °CISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 51.0 °CISO 75-1/-2
Vicat Softening Point 75.0 °C50°C/h, 50N; ISO 306
 177 °C50°C/h 10N; ISO 306
Brittleness Temperature -80.0 °CISO 974
Glass Transition Temp, Tg -25.0 °C10°C/min; ISO 11357-1/-2
Flammability, UL94 HB
@Thickness 1.50 mm
IEC 60695-11-10
 HB
@Thickness 3.00 mm
IEC 60695-11-10
Oxygen Index 20 %ISO 4589-1/-2
 
Processing PropertiesOriginal ValueComments
Melt Temperature 225 °COptimum, Extrusion
 220 - 235 °CRange, Extrusion
 230 °COptimum, Injection
 220 - 250 °CRange, Injection
Mold Temperature 45.0 °COptimum, Injection
 45.0 - 55.0 °CInjection
Drying Temperature 100 °CInjection
 90.0 - 110 °CExtrusion
Dry Time 2.00 - 3.00 hourExtrusion, Dehumidified Dryer
 2.00 - 3.00 hourInjection, Dehumidified Dryer
Moisture Content <= 0.060 %Extrusion
 <= 0.080 %Injection
 
Descriptive Properties
Drying RecommendedyesInjection
Eff. thermal diffusivity (m²/s)5.44E-08
FMVSS ClassSEISO 3795 (FMVSS 302)
Fogging (mg)0.1G-value (condensate); ISO 6452; DS
Part Marking Code>TPC-ET<ISO 11469
PolymerTPC
Resin IdentificationTPC-ETISO 1043

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Celanese Hytrel® 7246 TPC-ET
Celanese Hytrel® 5526 TPC-ET
Celanese Hytrel® G5544 TPC-ET
DuPont Mobility and Materials Hytrel® HTR8139BK TPC-ET
Celanese Hytrel® 6356 TPC-ET

PDSX5184 / 197824

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.