MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

SABIC LNP™ THERMOCOMP™ Compound LC008E Polyetheretherketone (PEEK) (Asia)
Categories: Polymer; Thermoplastic; Polyketone; Polyetheretherketone (PEEK)

Material Notes: LNP THERMOCOMP LC008E compound is based on Polyetheretherketone (PEEK) resin containing 40% carbon fiber. Added features of this grade include: Easy Molding, Electrically Conductive.

Features: High Stiffness,Light-weight Structural,High Heat Resistance,Super Strong (Carbon Fiber Filled),Electrically Conductive,Easy Molding,Structural

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.47 g/cc0.0531 lb/in³ASTM D792
 1.47 g/cc0.0531 lb/in³ISO 1183
Moisture Absorption 0.100 %0.100 %Injection Molding
Linear Mold Shrinkage, Flow 0.00050 cm/cm0.00050 in/in24hrs; ISO 294
 0.0010 - 0.0030 cm/cm0.0010 - 0.0030 in/in24hrs; ASTM D955
Linear Mold Shrinkage, Transverse 0.0060 - 0.0080 cm/cm0.0060 - 0.0080 in/in24hrs; ASTM D955
 0.0073 cm/cm0.0073 in/in24hrs; ISO 294
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 240 MPa34800 psiASTM D638
 242 MPa35100 psiISO 527
Elongation at Break 1.3 %1.3 %ASTM D638
 1.3 %1.3 %ISO 527
Tensile Modulus 30.52 GPa4427 ksi1 mm/min; ISO 527
 33.09 GPa4799 ksi5 mm/min; ASTM D638
Flexural Strength 352 MPa51100 psiISO 178
 365 MPa52900 psiASTM D790
Flexural Modulus 26.88 GPa3899 ksiASTM D790
 27.5 GPa3990 ksiISO 178
Izod Impact Notched 58.0 J42.8 ft-lbASTM D256
Izod Impact, Unnotched 7.04 J/cm13.2 ft-lb/inASTM D4812
Izod Impact, Notched (ISO) 5.00 kJ/m²2.38 ft-lb/in²80*10*4; ISO 180/1A
Izod Impact, Unnotched (ISO) 40.0 kJ/m²19.0 ft-lb/in²80*10*4; ISO 180/1U
Dart Drop, Total Energy 8.00 J5.90 ft-lbpeak; ASTM D3763
Impact Test 3.00 J2.21 ft-lbMultiaxial Impact; ISO 6603
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow  7.00 µm/m-°C
@Temperature -40.0 - 40.0 °C
3.89 µin/in-°F
@Temperature -40.0 - 104 °F
ISO 11359-2
 7.20 µm/m-°C
@Temperature -40.0 - 40.0 °C
4.00 µin/in-°F
@Temperature -40.0 - 104 °F
ASTM E831
CTE, linear, Transverse to Flow  27.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
15.0 µin/in-°F
@Temperature -40.0 - 104 °F
ASTM E831
 27.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
15.0 µin/in-°F
@Temperature -40.0 - 104 °F
ISO 11359-2
Deflection Temperature at 0.46 MPa (66 psi) 338 °C640 °FFlatw 80*10*4 sp=64mm; ISO 75/Bf
 338 °C
@Thickness 3.20 mm
640 °F
@Thickness 0.126 in
unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 326 °C619 °FFlatw 80*10*4 sp=64mm; ISO 75/Af
 322 °C
@Thickness 3.20 mm
612 °F
@Thickness 0.126 in
unannealed; ASTM D648
 
Processing PropertiesMetricEnglishComments
Zone 2 365 - 375 °C689 - 707 °F
Zone 3 380 - 395 °C716 - 743 °F
Melt Temperature 380 - 390 °C716 - 734 °FInjection Molding
Mold Temperature 140 - 165 °C284 - 329 °F
Drying Temperature 120 - 150 °C248 - 302 °FInjection Molding
Dry Time 4.00 hour4.00 hourInjection Molding
Back Pressure 0.300 - 0.700 MPa43.5 - 102 psi
Screw Speed 60 - 100 rpm60 - 100 rpm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PSABH81672 / 289619

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.