MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Leaded Nickel Brass, UNS C97300, Copper Casting Alloy, M01 Temper, As Sand Cast
Categories: Metal; Nonferrous Metal; Copper Alloy; Brass

Material Notes: Temper: As Sand Cast

Casting Characteristics: High – Drossing, Fluidity; Medium - Casting Yield, Effect of Section Size, Gassing, Shrinkage in Solidification

Fabrication Properties: Excellent Suitability – Soldering, Brazing

Typical uses: Ornamental Castings; Statuary; Hardware; Valves

Applicable Specifications: As Centrifugal Cast - Castings ASTM B271/B271M; As Continuous Cast – Castings SAE J461, Castings SAE J462, Castings ASTM B505/B505M; As Sand Cast – Castings ASTM B584, Castings ASTM B763/B763M; Ingot - ASTM B30

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 8.89 g/cc0.321 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 55
@Load 500 kg
55
@Load 1100 lb
Tensile Strength >= 207 MPa>= 30000 psifor Standard
 241 MPa35000 psiTypical
Tensile Strength, Yield >= 103 MPa>= 15000 psifor Standard, 0.5% Ext
 117 MPa17000 psiTypical, 0.5% Ext
Elongation at Break >= 8.0 %>= 8.0 %for Standard
 20 %20 %Typical
Tensile Modulus 110 GPa16000 ksi
Machinability 70 %70 %
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000290 ohm-cm0.0000290 ohm-cm6% IACS
 
Thermal PropertiesMetricEnglishComments
CTE, linear 16.2 µm/m-°C
@Temperature 20.0 - 300 °C
9.00 µin/in-°F
@Temperature 68.0 - 572 °F
Specific Heat Capacity 0.377 J/g-°C0.0900 BTU/lb-°F
Thermal Conductivity 2.38 W/m-K16.5 BTU-in/hr-ft²-°F
Melting Point 1010 - 1040 °C1850 - 1904 °F
Solidus 1010 °C1850 °F
Liquidus 1040 °C1904 °F
Shrinkage 1.56 %1.56 %Patternmaker's Shrinkage (3/16 in./ft.)
 
Processing PropertiesMetricEnglishComments
Processing Temperature 260 °C500 °FStress Relief
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al <= 0.0050 %<= 0.0050 %
Antimony, Sb <= 0.35 %<= 0.35 %
Copper, Cu 53 - 58 %53 - 58 %
Iron, Fe <= 1.5 %<= 1.5 %
Lead, Pb 8.0 - 11 %8.0 - 11 %
Manganese, Mn <= 0.50 %<= 0.50 %
Nickel, Ni 11 - 14 %11 - 14 %
Phosphorus, P <= 0.050 %<= 0.050 %
Silicon, Si <= 0.15 %<= 0.15 %
Sulfur, S <= 0.080 %<= 0.080 %
Tin, Sn 1.5 - 3.0 %1.5 - 3.0 %
Zinc, Zn 17 - 25 %17 - 25 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

MC97300x3 / 293257

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.