Sumitomo Bakelite Vyncolit® A2740 Phenolic Novolac
Categories:
Polymer
;
Thermoset
;
Phenolic
;
Phenolic, Novolac, Glass Filled
Material Notes:
Vyncolit® A2740 is a glass fiber reinforced phenolic molding compound with good thermal, electrical and mechanical properties.
Information provided by Sumitomo Bakelite High Performance Plastics (sbhpp)
Key Words:
PF-(GF+GB)55
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Density
1.71
g/cc
0.0618
lb/in³
ISO 1183
Apparent Bulk Density
0.650
g/cc
0.0235
lb/in³
ISO 60
Water Absorption
0.060 %
0.060 %
ISO 62
Linear Mold Shrinkage
0.0024
cm/cm
0.0024
in/in
ISO 2577
Mechanical Properties
Metric
English
Comments
Tensile Strength
95.0
MPa
13800
psi
ISO 527-1
Elongation at Break
0.78 %
0.78 %
ISO 527-1
Tensile Modulus
15.0
GPa
2180
ksi
ISO 527-1
Flexural Strength
201
MPa
29200
psi
ISO 178
Flexural Modulus
14.0
GPa
2030
ksi
ISO 178
Flexural Strain at Break
1.53 %
1.53 %
ISO 178
Compressive Strength
272
MPa
39500
psi
ISO 604
Charpy Impact Unnotched
1.30
J/cm²
6.19
ft-lb/in²
ISO 179-1
Charpy Impact, Notched
0.400
J/cm²
1.90
ft-lb/in²
ISO 179-1
Electrical Properties
Metric
English
Comments
Dielectric Strength
40.0
kV/mm
1020
kV/in
IEC 60243-1
Thermal Properties
Metric
English
Comments
CTE, linear, Parallel to Flow
15.0
µm/m-°C
8.33
µin/in-°F
TMA
CTE, linear, Transverse to Flow
42.0
µm/m-°C
23.3
µin/in-°F
TMA
Deflection Temperature at 1.8 MPa (264 psi)
219
°C
426
°F
ISO 75 Af
Shrinkage
0.030 %
0.030 %
Post; ISO 2577
Descriptive Properties
Color
Black
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
PSUMIT492 / 194297
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
info@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.