MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Ovako S400* SB400D Steel, +AR
Categories: Metal; Ferrous Metal; Alloy Steel

Material Notes: General Information: Grade SB400D is a micro-alloyed steel for general purposes with specified mechanical properties and impact requirements. The material is delivered as rolled and suitable for welding. The mechanical properties may change if the material is heat-treated. Grade SB420 is a micro-alloyed steel for general purposes with specified mechanical properties and impact requirements. The material is delivered as rolled. The mechanical properties may change if the material is heat-treated.

Information provided by Ovako

Key Words: 2142
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.80 g/cc0.282 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell  160 - 180
@Thickness 10.0 - 15.0 mm
160 - 180
@Thickness 0.394 - 0.591 in
Flat bar
 160 - 200
@Thickness 15.0 - 30.0 mm
160 - 200
@Thickness 0.591 - 1.18 in
Flat bar
 160 - 200
@Thickness >=30.0 mm
160 - 200
@Thickness >=1.18 in
Flat bar
Tensile Strength  530 - 600 MPa
@Thickness 10.0 - 15.0 mm
76900 - 87000 psi
@Thickness 0.394 - 0.591 in
Flat bar
 530 - 600 MPa
@Thickness 15.0 - 30.0 mm
76900 - 87000 psi
@Thickness 0.591 - 1.18 in
Flat bar
 530 - 600 MPa
@Thickness >=30.0 mm
76900 - 87000 psi
@Thickness >=1.18 in
Flat bar
Tensile Strength, Yield  >= 400 MPa
@Thickness 15.0 - 30.0 mm
>= 58000 psi
@Thickness 0.591 - 1.18 in
Rel, Flat bar
 >= 400 MPa
@Thickness >=30.0 mm
>= 58000 psi
@Thickness >=1.18 in
Rel, Flat bar
 >= 420 MPa
@Thickness 10.0 - 15.0 mm
>= 60900 psi
@Thickness 0.394 - 0.591 in
Rel, Flat bar
Elongation at Break  20 %
@Thickness 10.0 - 15.0 mm
20 %
@Thickness 0.394 - 0.591 in
Flat bar
 20 %
@Thickness 15.0 - 30.0 mm
20 %
@Thickness 0.591 - 1.18 in
Flat bar
 20 %
@Thickness >=30.0 mm
20 %
@Thickness >=1.18 in
Flat bar
Modulus of Elasticity 210 GPa30500 ksi
Poissons Ratio 0.300.30
Shear Modulus 80.0 GPa11600 ksi
Impact Test  27.0 J
@Thickness 10.0 - 15.0 mm,
Temperature -20.0 °C
19.9 ft-lb
@Thickness 0.394 - 0.591 in,
Temperature -4.00 °F
Flat bar
 27.0 J
@Thickness 15.0 - 30.0 mm,
Temperature -20.0 °C
19.9 ft-lb
@Thickness 0.591 - 1.18 in,
Temperature -4.00 °F
Flat bar
 27.0 J
@Thickness >=30.0 mm,
Temperature -20.0 °C
19.9 ft-lb
@Thickness >=1.18 in,
Temperature -4.00 °F
Flat bar
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000200 - 0.00000250 ohm-cm0.00000200 - 0.00000250 ohm-cm
 
Thermal PropertiesMetricEnglishComments
CTE, linear 12.0 µm/m-°C
@Temperature 20.0 - 300 °C
6.67 µin/in-°F
@Temperature 68.0 - 572 °F
Specific Heat Capacity 0.460 - 0.480 J/g-°C
@Temperature 50.0 - 100 °C
0.110 - 0.115 BTU/lb-°F
@Temperature 122 - 212 °F
Thermal Conductivity 40.0 - 45.0 W/m-K278 - 312 BTU-in/hr-ft²-°FAmbient temperature
Transformation Temperature 400 °C752 °FMS
 720 °C1330 °FAC1
 820 °C1510 °FAC3
 
Component Elements PropertiesMetricEnglishComments
Carbon, C <= 0.20 %<= 0.20 %
Iron, Fe >= 97.61 %>= 97.61 %As Balance
Manganese, Mn <= 1.6 %<= 1.6 %
Nitrogen, N <= 0.020 %<= 0.020 %
Phosphorus, P <= 0.035 %<= 0.035 %
Silicon, Si <= 0.50 %<= 0.50 %
Sulfur, S <= 0.035 %<= 0.035 %
 
Descriptive Properties
WeldabilityCEV 0.48max
 Pcm 0.31max

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

NOVAKO423 / 234722

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.