MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Solvay CYCOM® 5250-4 RTM BMI Resin, Composite with IM7-6K-4HS Fabric
Categories: Polymer; Thermoset; Bismaleimide (BMI); Carbon Fiber/Thermoset Composite

Material Notes: CYCOM® 5250-4 RTM is a true one-part homogeneous BMI resin developed specifically for the resin transfer molding (RTM) process. It reaches very low viscosity during transfer and maintains a low viscosity for several hours, thus providing the maximum capability to fabricate complex parts. Laminates fabricated from CYCOM 5250-4 RTM are capable of service temperatures up to 400°F (204°C), but its toughness and processability make it an ideal material for 180°F (82°C) temperature applications where epoxies are commonly used. CYCOM 5250-4 RTM offers the highest open hole compression (OHC) value of any organic matrix resin while providing the highest level of toughness available in an RTM capable matrix resin.

Features & Benefits:

  • Excellent toughness
  • Maximum continuous service temperature up to 400°F (204°C)
  • Superior hot/wet properties at 160 to 375°F (71 to190°C)
  • Low viscosity during processing
  • Low-tack, solid at room temperature provides ease of handling
  • Low thermal conductivity
  • Versatile cure, can be cured at 400°F (204°C) for 2 hours
  • Out-time greater than 60 days at room temperature
  • True one-part formulation
  • Fully compatible CYCOM 5240-4 RTM low resin content prepregs and CYCOM 782 RTM bindercoated fabrics are available for preform manufacture
Applications:
  • Wing stabilizer spars
  • Fuselage skins and stiffeners
  • Low operating temperature, critical load-bearing components
  • Engine components
Mechanical properties for composites with 58% fiber volume IM7-6K-4HS carbon fiber fabric, after standard cure + postcure unless otherwise noted.

Information provided by Cytec, subsequently acquired by Solvay.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Water Absorption 3.9 %
@Temperature 71.1 °C,
Time 3.60e+6 sec
Neat resin after 400°F cure (no postcure)
 4.2 %
@Temperature 71.1 °C,
Time 3.60e+6 sec
Neat resin after standard cure + postcure
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength 70000 psi
@Temperature 177 °C
Open hole, wet
 77000 psi
@Temperature 24.0 °C
Open hole
Tensile Modulus 72.0 GPa
@Temperature 24.0 °C
Open hole
 79.0 GPa
@Temperature 177 °C
Open hole, wet
Flexural Strength 88000 psi
@Temperature 177 °C
Fill 90° Direction, wet
 91000 psi
@Temperature 177 °C
Warp 0° Direction, wet
 150000 psi
@Temperature 25.0 °C
Fill 90° Direction
 160000 psi
@Temperature 2.00 °C
Warp 0° Direction
Flexural Modulus 67.6 GPa
@Temperature 177 °C
Fill 90° Direction, wet
 69.7 GPa
@Temperature 25.0 °C
Fill 90° Direction
 72.4 GPa
@Temperature 177 °C
Warp 0° Direction, wet
 72.4 GPa
@Temperature 2.00 °C
Warp 0° Direction
Compressive Strength 179 MPaCure 350°F (177°C) for 6 hours, 216° C Tg, after Impact 1500 in-lb/in
 186 MPaCure 470°F (243°C) for 6 hours, 293° C Tg, after Impact 1500 in-lb/in
 193 MPaCure 440°F (227°C) for 6 hours, 282° C Tg, after Impact 1500 in-lb/in
 214 MPaCure 375°F (191°C) for 4 hours, 249° C Tg, after Impact 1500 in-lb/in
 220 MPaafter 1500 in-lb/in impact
 221 MPaCure 400°F (204°C) for 2 hours, 252° C Tg, after Impact 1500 in-lb/in
 221 MPaCure 410°F (210°C) for 6 hours, 263° C Tg, after Impact 1500 in-lb/in
Shear Strength 6100 psi
@Thickness 4500 mm
Short beam, Warp 0° Direction, wet
 12000 psi
@Thickness 50.8 mm
Short beam, Warp 0° Direction
 
Thermal PropertiesOriginal ValueComments
Maximum Service Temperature, Air 204 °Ccontinuous
Glass Transition Temp, Tg 199 °CCure 204°C for 2 hrs-no postcure, wet
 207 °CStandard Cure+Standard Postcure, wet
 254 °CCure 204°C for 2 hrs-no postcure, dry
 271 °CStandard Cure+Standard Postcure, dry
 
Processing PropertiesOriginal ValueComments
Processing Temperature 350 - 375 °F
@Time 21600 sec
Standard Cure. Standard post cure is 440°F for 4 hours
 <= 400 °F
@Time 7200 sec
optional cure (no postcure)
Gel Time 35.0 min
@Temperature 177 °C
Shelf Life 6.00 Month
@Temperature <=-17.8 °C
sealed container

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Solvay CYCOM® 5250-4 RTM BMI Resin, Composite with T650-35-3K-PW Fabric
Solvay CYCOM® 381 Epoxy Prepreg with IM7 Uni-graphite and 148FAW Epoxy
Solvay CYCOM® 5320-1 Epoxy with T40/800B Unidirectional Tape Composite
Solvay CYCOM® 890 RTM Resin - Woven Carbon Fabric Composite
Solvay CYCOM® 977-3 Epoxy - Unidirectional Carbon Fiber Tape

PCYTED079b / 233832

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.