MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Eneos NV75G NBR/PVC
Categories: Polymer; Thermoset; Rubber or Thermoset Elastomer (TSE)

Material Notes: SR NV is polymer alloy of NBR and polyvinyl chloride (abbrevia ted as“ PVC” below) that offers high oil and fuel oil resistance as well as excellent ozone resistance.

ENEOS has acquired the elastomer product lines from JSR Corporation.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Mooney Viscosity  68
@Temperature 100 °C
68
@Temperature 212 °F
ML1+4
 72
@Temperature 100 °C
72
@Temperature 212 °F
ML1+4, Compound (non-vulcanized)
 46
@Temperature 125 °C,
Time 61200 sec
46
@Temperature 257 °F,
Time 17.0 hour
Scorch Test, ML1, Compound (non-vulcanized)
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 8282Compound (vulcanized)
 66
@Temperature 40.0 °C,
Time 173000 sec
66
@Temperature 104 °F,
Time 48.0 hour
Fuel Oil B, Compound (non-vulcanized)
 71
@Temperature 120 °C,
Time 252000 sec
71
@Temperature 248 °F,
Time 70.0 hour
IRM903, Compound (vulcanized)
 85
@Temperature 120 °C,
Time 252000 sec
85
@Temperature 248 °F,
Time 70.0 hour
Air heat Aging, Compound (non-vulcanized)
 87
@Temperature 120 °C,
Time 252000 sec
87
@Temperature 248 °F,
Time 70.0 hour
IRM901, Compound (vulcanized)
Tensile Strength 20.6 MPa2990 psiCompound (vulcanized)
 12.978 MPa
@Temperature 40.0 °C,
Time 173000 sec
1882.3 psi
@Temperature 104 °F,
Time 48.0 hour
Fuel Oil B, Compound (non-vulcanized)
 17.922 MPa
@Temperature 120 °C,
Time 252000 sec
2599.4 psi
@Temperature 248 °F,
Time 70.0 hour
IRM903, Compound (vulcanized)
 22.248 MPa
@Temperature 120 °C,
Time 252000 sec
3226.8 psi
@Temperature 248 °F,
Time 70.0 hour
Air heat Aging, Compound (non-vulcanized)
 22.866 MPa
@Temperature 120 °C,
Time 252000 sec
3316.4 psi
@Temperature 248 °F,
Time 70.0 hour
IRM901, Compound (vulcanized)
Elongation at Break 370 %370 %Compound (vulcanized)
 214.6 %
@Temperature 120 °C,
Time 252000 sec
214.6 %
@Temperature 248 °F,
Time 70.0 hour
IRM901, Compound (vulcanized)
 251.6 %
@Temperature 120 °C,
Time 252000 sec
251.6 %
@Temperature 248 °F,
Time 70.0 hour
Air heat Aging, Compound (non-vulcanized)
 255.3 %
@Temperature 40.0 °C,
Time 173000 sec
255.3 %
@Temperature 104 °F,
Time 48.0 hour
Fuel Oil B, Compound (non-vulcanized)
 292.3 %
@Temperature 120 °C,
Time 252000 sec
292.3 %
@Temperature 248 °F,
Time 70.0 hour
IRM903, Compound (vulcanized)
100% Modulus 10.5 MPa1520 psiCompound (vulcanized)
300% Modulus 19.0 MPa2760 psiCompound (vulcanized)
Resilience 2222[%], Rebound, Compound (vulcanized)
Tear Strength 53.0 kN/m302 pliCompound (vulcanized)
Compression Set  32 %
@Temperature 100 °C,
Time 252000 sec
32 %
@Temperature 212 °F,
Time 70.0 hour
Compound (vulcanized)
 44 %
@Temperature 120 °C,
Time 252000 sec
44 %
@Temperature 248 °F,
Time 70.0 hour
Compound (vulcanized)
 
Thermal PropertiesMetricEnglishComments
Brittleness Temperature -29.0 °C-20.2 °F
 
Descriptive Properties
Acrylonitrile ContentMedium
Delta;V100 (%)2Distilled Water 70 hr at 40°C, Compound (non-vulcanized)
 20Fuel Oil B 48 hrs at 40°C, Compound (non-vulcanized)
 42Fuel Oil C 48 hrs at 40°C, Compound (non-vulcanized)
 64Fuel Oil C/Ethanol 48 hrs at 40°C, Compound (non-vulcanized)
 7IRM903 70 hrs at 120°C, Compound (vulcanized)
 -9IRM901 70 hrs at 120°C, Compound (vulcanized)
Extrusion Test402 cc/min80°C, 25 rpm, Extrusion Volume
 4680°C, 25 rpm, Die Swell %
 550 cm/min80°C, 25 rpm, Extrusion Length
Flex Test2Growth 2 to 15 mm (Thousand Times)
 20Occurrence(Thousand Times)
Flow Rate105Q×104, 80°C, 100 kg, Kokahiki Flow tester
JSR Mold Curast Test 160°C, Minutes3tc(10)
 5tc(90)
Low-Temperature Torsion Test-20°Ct10
 -34°Ct100
Mill Contraction 50°C (%)20
NBR/PVC70/30
Ozone Degradability TestNCStatic 20% Elongation, 50 ppm 5 Hours at 40°C
 NCDynamic 0 to 20% Elongation, 50 ppm 5 Hours at 40°C
Product formSheet
Product StainSS

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PJSRC8082 / 295398

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.