MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

LG Chemical SBR 1712 High Acrylonitrile Polymer
Categories: Polymer; Thermoset; Rubber or Thermoset Elastomer (TSE)

Material Notes: Description: SBR 1712 is an oil extended cold polymerization SBR with 37.5 parts of highly aromatic oil and styrene-butadiene copolymer of 23.5% bound styrene. Raw materials for this product are carefully chosen for the best physical properties. The highly aromatic oil in SBR 1712 is a efficient plasticizer for high molecular weight SBR and it result in superior physical and processing properties compared to the other type of oil.

Applications: SBR 1712 is produced to meet a rigid APF (Assured Processability Factor) and can be used to tire, camelback and other industrial products for the dark colored goods.

CAS No: 9003-55-8

Information provided by LG Chemical

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 0.950 g/cc0.950 g/cc
Volatiles 0.20 %0.20 %
Mooney Viscosity 49
@Temperature 100 °C
49
@Temperature 212 °F
ML 1+4
Ash 0.20 %0.20 %
 
Chemical PropertiesMetricEnglishComments
Styrene Content 23.5 %23.5 %Bound
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 24.0 MPa
@Treatment Temp. 145 °C,
Time 2100 sec
3480 psi
@Treatment Temp. 293 °F,
Time 0.583 hour
ASTM D412
Elongation at Break 600 %
@Treatment Temp. 145 °C,
Time 2100 sec
600 %
@Treatment Temp. 293 °F,
Time 0.583 hour
ASTM D412
300% Modulus 10.3 MPa
@Treatment Temp. 145 °C,
Time 2100 sec
1490 psi
@Treatment Temp. 293 °F,
Time 0.583 hour
ASTM D412
 
Descriptive Properties
ColorDark Brown Bale
ComponentsHAF68.75, ASTM D3185
 SBR 1712137.5, ASTM D3185
 Stearic Acid1, ASTM D3185
 Sulfur1.75, ASTM D3185
 TBBS1.38, ASTM D3185
 ZnO3, ASTM D3185
Oil Analysis27.3%
Organic Acid5%
Rheometer15.0 mint'90, 160°C, 1° Arc, ASTM D5289
 20 lb-inMH, 160°C, 1° Arc, ASTM D5289
 3.3 lb-inML, 160°C, 1° Arc, ASTM D5289
 5.2 mints1, 160°C, 1° Arc, ASTM D5289
 9.0 mint'50, 160°C, 1° Arc, ASTM D5289
Soap0.1%

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
LG Chemical HI-121 ABS, High Impact

PLAY746 / 148756

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.