Physical Properties | Metric | English | Comments |
---|
Specific Gravity | 4.46 g/cc | 4.46 g/cc |
|
Chemical Properties | Metric | English | Comments |
---|
Acid Class, SR | 4.0 | 4.0 |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Knoop | 730 @Load 0.0999 kg | 730 @Load 0.220 lb |
Modulus of Elasticity | 122.3 GPa | 17740 ksi |
Modulus of Rigidity | 47.1 GPa | 6830 ksi |
Poissons Ratio | 0.30 | 0.30 |
Abrasion | 61 | 61 |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear | 6.10 µm/m-°C @Temperature -30.0 - 70.0 °C | 3.39 µin/in-°F @Temperature -22.0 - 158 °F |
| 7.50 µm/m-°C @Temperature 100 - 300 °C | 4.17 µin/in-°F @Temperature 212 - 572 °F |
Thermal Conductivity | 0.856 W/m-K @Temperature 35.0 °C | 5.94 BTU-in/hr-ft²-°F @Temperature 95.0 °F |
Transformation Temperature, Tg | 691 °C | 1280 °F |
Softening Point | 745 °C | 1370 °F |
Annealing Point | 677 °C | 1250 °F |
Strain Point | 648 °C | 1200 °F |
|
Optical Properties | Metric | English | Comments |
---|
Refractive Index | 1.76127 @Wavelength 2325.42 nm | 1.76127 @Wavelength 2325.42 nm |
| 1.76833 @Wavelength 1970.09 nm | 1.76833 @Wavelength 1970.09 nm |
| 1.77597 @Wavelength 1529.58 nm | 1.77597 @Wavelength 1529.58 nm |
| 1.78303 @Wavelength 1128.64 nm | 1.78303 @Wavelength 1128.64 nm |
| 1.78548 @Wavelength 1013.98 nm | 1.78548 @Wavelength 1013.98 nm |
| 1.78991 @Wavelength 852.11 nm | 1.78991 @Wavelength 852.11 nm |
| 1.79302 @Wavelength 768.19 nm | 1.79302 @Wavelength 768.19 nm |
| 1.7959 @Wavelength 706.52 nm | 1.7959 @Wavelength 706.52 nm |
| 1.79882 @Wavelength 656.27 nm | 1.79882 @Wavelength 656.27 nm |
| 1.79964 @Wavelength 643.85 nm | 1.79964 @Wavelength 643.85 nm |
| 1.8004 @Wavelength 632.8 nm | 1.8004 @Wavelength 632.8 nm |
| 1.80385 @Wavelength 589.29 nm | 1.80385 @Wavelength 589.29 nm |
| 1.804 @Wavelength 587.56 nm | 1.804 @Wavelength 587.56 nm |
| 1.80811 @Wavelength 546.07 nm | 1.80811 @Wavelength 546.07 nm |
| 1.8161 @Wavelength 486.13 nm | 1.8161 @Wavelength 486.13 nm |
| 1.8171 @Wavelength 479.99 nm | 1.8171 @Wavelength 479.99 nm |
| 1.82445 @Wavelength 441.57 nm | 1.82445 @Wavelength 441.57 nm |
| 1.82573 @Wavelength 435.835 nm | 1.82573 @Wavelength 435.835 nm |
| 1.83385 @Wavelength 404.656 nm | 1.83385 @Wavelength 404.656 nm |
| 1.84792 @Wavelength 365.015 nm | 1.84792 @Wavelength 365.015 nm |
Abbe Number | 46.28 | 46.28 |
| 46.53 | 46.53 |
Optical Dispersion | 0.005184 | 0.005184 |
| 0.005801 | 0.005801 |
| 0.008114 | 0.008114 |
| 0.008476 | 0.008476 |
| 0.008987 | 0.008987 |
| 0.009296 | 0.009296 |
| 0.009637 | 0.009637 |
| 0.013334 | 0.013334 |
| 0.014154 | 0.014154 |
| 0.017281 | 0.017281 |
| 0.017463 | 0.017463 |
| 0.021734 | 0.021734 |
| 0.022188 | 0.022188 |
| 0.030823 | 0.030823 |
Transmission, Visible | 95.7 % @Thickness 10.0 mm, Wavelength 380 nm | 95.7 % @Thickness 0.394 in, Wavelength 380 nm |
| 97.1 % @Thickness 10.0 mm, Wavelength 390 nm | 97.1 % @Thickness 0.394 in, Wavelength 390 nm |
| 97.9 % @Thickness 10.0 mm, Wavelength 400 nm | 97.9 % @Thickness 0.394 in, Wavelength 400 nm |
| 98.7 % @Thickness 10.0 mm, Wavelength 420 nm | 98.7 % @Thickness 0.394 in, Wavelength 420 nm |
| 99.1 % @Thickness 10.0 mm, Wavelength 440 nm | 99.1 % @Thickness 0.394 in, Wavelength 440 nm |
| 99.3 % @Thickness 10.0 mm, Wavelength 460 nm | 99.3 % @Thickness 0.394 in, Wavelength 460 nm |
| 99.6 % @Thickness 10.0 mm, Wavelength 480 nm | 99.6 % @Thickness 0.394 in, Wavelength 480 nm |
| 99.7 % @Thickness 10.0 mm, Wavelength 500 nm | 99.7 % @Thickness 0.394 in, Wavelength 500 nm |
| 99.9 % @Thickness 10.0 mm, Wavelength 550 nm | 99.9 % @Thickness 0.394 in, Wavelength 550 nm |
| 99.9 % @Thickness 10.0 mm, Wavelength 600 nm | 99.9 % @Thickness 0.394 in, Wavelength 600 nm |
| 99.9 % @Thickness 10.0 mm, Wavelength 650 nm | 99.9 % @Thickness 0.394 in, Wavelength 650 nm |
| 99.9 % @Thickness 10.0 mm, Wavelength 700 nm | 99.9 % @Thickness 0.394 in, Wavelength 700 nm |
IR Transmittance | 72 % @Thickness 10.0 mm, Wavelength 2400 nm | 72 % @Thickness 0.394 in, Wavelength 2400 nm |
| 91.6 % @Thickness 10.0 mm, Wavelength 2200 nm | 91.6 % @Thickness 0.394 in, Wavelength 2200 nm |
| 96.8 % @Thickness 10.0 mm, Wavelength 2000 nm | 96.8 % @Thickness 0.394 in, Wavelength 2000 nm |
| 98.9 % @Thickness 10.0 mm, Wavelength 1800 nm | 98.9 % @Thickness 0.394 in, Wavelength 1800 nm |
| 99.6 % @Thickness 10.0 mm, Wavelength 1600 nm | 99.6 % @Thickness 0.394 in, Wavelength 1600 nm |
| 99.8 % @Thickness 10.0 mm, Wavelength 1400 nm | 99.8 % @Thickness 0.394 in, Wavelength 1400 nm |
| 99.9 % @Thickness 10.0 mm, Wavelength 800 nm | 99.9 % @Thickness 0.394 in, Wavelength 800 nm |
| 99.9 % @Thickness 10.0 mm, Wavelength 900 nm | 99.9 % @Thickness 0.394 in, Wavelength 900 nm |
| 99.9 % @Thickness 10.0 mm, Wavelength 1000 nm | 99.9 % @Thickness 0.394 in, Wavelength 1000 nm |
| 99.9 % @Thickness 10.0 mm, Wavelength 1200 nm | 99.9 % @Thickness 0.394 in, Wavelength 1200 nm |
UV Transmittance | 5.0 % @Thickness 10.0 mm, Wavelength 310 nm | 5.0 % @Thickness 0.394 in, Wavelength 310 nm |
| 25 % @Thickness 10.0 mm, Wavelength 320 nm | 25 % @Thickness 0.394 in, Wavelength 320 nm |
| 53 % @Thickness 10.0 mm, Wavelength 330 nm | 53 % @Thickness 0.394 in, Wavelength 330 nm |
| 72 % @Thickness 10.0 mm, Wavelength 340 nm | 72 % @Thickness 0.394 in, Wavelength 340 nm |
| 83 % @Thickness 10.0 mm, Wavelength 350 nm | 83 % @Thickness 0.394 in, Wavelength 350 nm |
| 89 % @Thickness 10.0 mm, Wavelength 360 nm | 89 % @Thickness 0.394 in, Wavelength 360 nm |
| 93.4 % @Thickness 10.0 mm, Wavelength 370 nm | 93.4 % @Thickness 0.394 in, Wavelength 370 nm |
|
Descriptive Properties |
---|
Acid Resistance, Powder Method, RA(P) | 3 |
CCI | 0.00 B |
| 0.4 G |
| 0.4 R |
coloring, λ 5 | 310 |
coloring, λ 80 | 380 |
Coloring, Internal Transmission λ 0.05 | 310 |
Coloring, Internal Transmission λ 0.80 | 347 |
Knoop Hardness Class | 7 |
Ohara Code d | 804465 |
Ohara Code e | 808463 |
Phosphate Resistance, PR | 1 |
Photoelastic Constant (ß) | 1.27 |
Water Resistance, RW(P) | 1 |
Weathering Resistance (Surface Method) W(S)max | 2 |
Yield Point, At (°C) | 720 |