MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
Pressure Seal 23811 Ethylene Propylene
Categories: Polymer; Thermoset; Rubber or Thermoset Elastomer (TSE)

Material Notes: Compound 23811 is an 80 durometer black colored EPDM elastomer, it is formulated for use with acids and alkalis with the exception of concentrated Nitric and Sulfuric acid. It exhibits excellent resistance to heat, compression set and automotive brake fluid. It will remain non brittle at very low temperatures. It also demonstrates excellent weathering and steam properties. This compound will meet or exceed the specifications listed and has the following physical properties: ASTM D2000 2 AA 815 A13 C12 F17 EA14; 2 BA 815 C12 F17; 4 BA 815 A14 C12 F17; 7 BA 810 C12; 6 CA 810 A25 B35 C32 F17 EA14; 7 CA 815 A25 B35 C32 F17 F18 EA14; 8 CA 815 A25 B35 C32 F19 G11 G21; 2 DA 815 A26 B36 C32 F19 G11 G21 EA14; 3 DA 815 A26 B36 C32 F19 G11 G21 EA14

Information provided by Pressure Seals Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.11 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 81
 70
@Treatment Temp. 23.0 °C,
Time 252000 sec
Methanol
 71
@Treatment Temp. 23.0 °C,
Time 252000 sec
Hydrochloric Acid
 76
@Treatment Temp. 23.0 °C,
Time 252000 sec
Methyl Ethyl Ketone
 79
@Treatment Temp. 120 °C,
Time 252000 sec
SAE Compatibility Fluid
 80
@Treatment Temp. 120 °C,
Time 252000 sec
DOT #3 Brake Fluid
 80
@Treatment Temp. 120 °C,
Time 252000 sec
DOT #5 Brake Fluid
 80
@Treatment Temp. 23.0 °C,
Time 252000 sec
Nitric Acid
 81
@Treatment Temp. 23.0 °C,
Time 252000 sec
Sodium Hydroxide
 81
@Treatment Temp. 100 °C,
Time 252000 sec
Distilled water aged
 83
@Treatment Temp. 125 °C,
Time 252000 sec
Heat Aged, Test Tube Method
 83
@Treatment Temp. 70.0 °C,
Time 252000 sec
Heat Aged
 83
@Treatment Temp. 100 °C,
Time 252000 sec
Heat Aged
 83
@Treatment Temp. 125 °C,
Time 252000 sec
Heat Aged
 84
@Treatment Temp. 150 °C,
Time 252000 sec
Heat Aged
 84
@Treatment Temp. 150 °C,
Time 252000 sec
Heat Aged, Test Tube Method
Tensile Strength 2019 psi
 1617.2 psi
@Treatment Temp. 23.0 °C,
Time 252000 sec
Methyl Ethyl Ketone
 1835.2 psi
@Treatment Temp. 23.0 °C,
Time 252000 sec
Nitric Acid
 1839.3 psi
@Treatment Temp. 120 °C,
Time 252000 sec
DOT #3 Brake Fluid
 1859.5 psi
@Treatment Temp. 23.0 °C,
Time 252000 sec
Sodium Hydroxide
 1879.7 psi
@Treatment Temp. 120 °C,
Time 252000 sec
SAE Compatibility Fluid
 1897.9 psi
@Treatment Temp. 125 °C,
Time 252000 sec
Heat Aged, Test Tube Method
 1897.9 psi
@Treatment Temp. 125 °C,
Time 252000 sec
Heat Aged
 1918 psi
@Treatment Temp. 23.0 °C,
Time 252000 sec
Methanol
 1928.1 psi
@Treatment Temp. 100 °C,
Time 252000 sec
Distilled water aged
 1944.3 psi
@Treatment Temp. 120 °C,
Time 252000 sec
DOT #5 Brake Fluid
 1978.6 psi
@Treatment Temp. 100 °C,
Time 252000 sec
Heat Aged
 2053.3 psi
@Treatment Temp. 70.0 °C,
Time 252000 sec
Heat Aged
 2073.5 psi
@Treatment Temp. 150 °C,
Time 252000 sec
Heat Aged
 2073.5 psi
@Treatment Temp. 150 °C,
Time 252000 sec
Heat Aged, Test Tube Method
 2140.1 psi
@Treatment Temp. 23.0 °C,
Time 252000 sec
Hydrochloric Acid
Elongation, Ultimate 221 %
 170.9 %
@Treatment Temp. 120 °C,
Time 252000 sec
SAE Compatibility Fluid
 194.1 %
@Treatment Temp. 125 °C,
Time 252000 sec
Heat Aged
 194.1 %
@Treatment Temp. 125 °C,
Time 252000 sec
Heat Aged, Test Tube Method
 196.9 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
Sodium Hydroxide
 204 %
@Treatment Temp. 100 °C,
Time 252000 sec
Heat Aged
 208 %
@Treatment Temp. 70.0 °C,
Time 252000 sec
Heat Aged
 208 %
@Treatment Temp. 120 °C,
Time 252000 sec
DOT #3 Brake Fluid
 208 %
@Treatment Temp. 120 °C,
Time 252000 sec
DOT #5 Brake Fluid
 211.9 %
@Treatment Temp. 100 °C,
Time 252000 sec
Distilled water aged
 211.9 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
Methanol
 215 %
@Treatment Temp. 150 °C,
Time 252000 sec
Heat Aged
 215 %
@Treatment Temp. 150 °C,
Time 252000 sec
Heat Aged, Test Tube Method
 225 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
Hydrochloric Acid
 230.1 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
Nitric Acid
 259.9 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
Methyl Ethyl Ketone
100% Modulus 875 psi
Tear Strength 162 pliDie B
 181 pliDie C
Compression Set 5.5 %
@Treatment Temp. 125 °C,
Time 79200 sec
Solid
 6.4 %
@Treatment Temp. 70.0 °C,
Time 79200 sec
Solid
 7.0 %
@Treatment Temp. 100 °C,
Time 252000 sec
Solid
 8.1 %
@Treatment Temp. 70.0 °C,
Time 79200 sec
Plied
 8.4 %
@Treatment Temp. 100 °C,
Time 79200 sec
Solid
 9.9 %
@Treatment Temp. 100 °C,
Time 252000 sec
Plied
 10.2 %
@Treatment Temp. 100 °C,
Time 79200 sec
Plied
 11 %
@Treatment Temp. 125 °C,
Time 79200 sec
Plied
 14.3 %
@Treatment Temp. 150 °C,
Time 79200 sec
Plied
 
Thermal PropertiesOriginal ValueComments
Brittleness Temperature <= -76.0 °F
Shrinkage 0.10 %
@Treatment Temp. 100 °C,
Time 252000 sec
Volume, Distilled water aged
 0.30 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
Volume, Sodium Hydroxide
 0.30 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
Volume, Methanol
 1.6 %
@Treatment Temp. 120 °C,
Time 252000 sec
Volume, SAE Compatibility Fluid
 2.1 %
@Treatment Temp. 120 °C,
Time 252000 sec
Volume, DOT #3 Brake Fluid
 3.1 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
Volume, Hydrochloric Acid
 3.6 %
@Treatment Temp. 120 °C,
Time 252000 sec
Volume, DOT #5 Brake Fluid
 7.3 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
Volume, Nitric Acid
 11.3 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
Volume, Methyl Ethyl Ketone
 
Descriptive Properties
ColorBlack

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PPRESL233 / 318443

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.