MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Syensqo (Solvay Specialty Polymers) Amodel® A-1625 HS PPA, 25% carbon/glass fiber
Categories: Polymer; Thermoplastic; Polyphthalamide (PPA)

Material Notes: 25% carbon/glass fiber, ESD grade, heat stabilized

Amodel® A-1625 HS is a carbon and glass-reinforced, heat-stabilized grade of polyphthalamide (PPA). It is formulated for applications requiring the dissipation of static charge. This material is well suited for fuel systems applications requiring low permeation, low swell, and high thermal resistance. It can also be used for components of electrical/electronic systems requiring high strength and stiffness, as well as static charge dissipation.

Amodel® A-1625 HS provides low moisture absorption, excellent dimensional stability and has creep resistance superior to other electrostatic dissipative materials.

- Black: A-1625 HS BK 324

Markets/Uses: Automotive / Automotive E/E / Electric Vehicles; Engine Sensors; EV Recharger Connectors; Sensors; Fuel Systems / Fuel Flanges; Quick Connects

Applications: Automotive Applications; Automotive Electronics; Automotive Under the Hood; Connectors; Electrical/Electronic Applications; Fuel Lines

Features: Chemical Resistant; Creep Resistant; Good Dimensional Stability; Good Stiffness; High Heat Resistance; High Stiffness; High Temperature Strength; Low Moisture Absorption

Injection notes: Storage:
- Amodel® compounds are shipped in moisture-resistant packages at moisture levels according to specifications. Sealed, undamaged bags should be preferably stored in a dry room at a maximum temperature of 50°C (122°F) and should be protected from possible damage. If only a portion of a package is used, the remaining material should be transferred into a sealable container. It is recommended that Amodel® resins be dried prior to molding following the recommendations found in this datasheet and/or in the Amodel® processing guide.

Information provided by Solvay Specialty Polymers.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.32 g/cc0.0477 lb/in³Method A; ISO 1183
Water Absorption 0.32 %
@Thickness 50.8 mm,
Time 86400 sec
0.32 %
@Thickness 2.00 in,
Time 24.0 hour
ASTM D570
Linear Mold Shrinkage, Flow 0.0040 cm/cm0.0040 in/inISO 294-4
Linear Mold Shrinkage, Transverse 0.0060 cm/cm0.0060 in/inISO 294-4
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength 205 MPa29700 psiASTM D638
Elongation at Break 2.5 %2.5 %ASTM D638
Tensile Modulus 15.0 GPa2180 ksiISO 527-2
 15.2 GPa2200 ksiASTM D638
Flexural Strength 300 MPa43500 psiISO 178
Flexural Modulus 13.5 GPa1960 ksiISO 178
Izod Impact, Notched 1.20 J/cm2.25 ft-lb/inASTM D256
Izod Impact, Notched (ISO) 8.00 kJ/m²3.81 ft-lb/in²ISO 180
Izod Impact, Unnotched (ISO)  50.0 kJ/m²
@Temperature -40.0 °C
23.8 ft-lb/in²
@Temperature -40.0 °F
ISO 180
 50.0 kJ/m²
@Temperature 23.0 °C
23.8 ft-lb/in²
@Temperature 73.4 °F
ISO 180
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 2400 ohm-cm2400 ohm-cmASTM D257
 20000 ohm-cm20000 ohm-cmIEC 62631-3-1
 200000 ohm-cm200000 ohm-cmIEC 62631-3-1
 
Thermal PropertiesMetricEnglishComments
Melting Point 310 °C590 °FISO 11357-3
 310 °C590 °FDSC
Deflection Temperature at 0.46 MPa (66 psi) 285 °C545 °FUnannealed; ISO 75-2/B
Deflection Temperature at 1.8 MPa (264 psi) 270 °C518 °FUnannealed; ASTM D648
 275 °C527 °FUnannealed; ISO 75-2/A
 
Processing PropertiesMetricEnglishComments
Rear Barrel Temperature 310 °C590 °F
Front Barrel Temperature 320 °C608 °F
Melt Temperature 320 - 330 °C608 - 626 °FInjection
Mold Temperature 135 °C275 °F
Drying Temperature 120 °C
@Time 14400 sec
248 °F
@Time 4.00 hour
Moisture Content 0.030 - 0.060 %0.030 - 0.060 %Injection
 
Descriptive Properties
AdditiveHeat Stabilizer
AvailabilityAsia Pacific
 Europe
 Latin America
 North America
ColorBlack
FormsPellets
ProcessingInjection Molding

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PSOL8Y4048 / 279848

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.