MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Carbon-Core CarbonFoam PU 4 R PU
Categories: Polymer; Thermoset; Polyurethane, TS; Thermoset Polyurethane Foam, Unreinforced

Material Notes: Standard sheet size is 48” X96”
All CarbonFoam PU products can be supplied in customer specified CNC cut kit form.
Closed cell content up to 95%
Freeze and thaw cycle tested.
Anti-static additives available for specific applications.
Low-abrasion additives available for machining applications.
Fire - retardant additives available.

Information provided by Carbon-Core

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Water Absorption 0.060 %0.060 %ASTM C272
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength 0.379 MPa55.0 psiASTM D1623
Tensile Modulus 0.0159 GPa2.30 ksiASTM D1623
Flexural Strength 0.883 MPa128 psiASTM D790
Compressive Strength 0.552 MPa80.0 psiPerpendicular to ruse-width; ASTM D1621
 0.655 MPa95.0 psiparallel to rise-thickness; ASTM D1621
 0.689 MPa100 psiPerpendicular to rise-length; ASTM D1621
Compressive Modulus 0.0124 GPa1.80 ksiPerpendicular to ruse-width; ASTM D1621
 0.0145 GPa2.10 ksiASTM D1621
 0.0179 GPa2.60 ksiPerpendicular to rise-length; ASTM D1621
Shear Modulus 0.00448 GPa0.650 ksiASTM C273
Shear Strength 0.290 MPa42.0 psiASTM C273
 
Electrical PropertiesMetricEnglishComments
Dielectric Constant 1.31.3
 
Thermal PropertiesMetricEnglishComments
Thermal Conductivity 0.0274 W/m-K0.190 BTU-in/hr-ft²-°FK-Factor
Insulation R Value 5.35.3
 
Descriptive Properties
Buoyancy57 lb/ft3
Closed Cell Rate0.95
Dimensional Stability-297-300°F

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Carbon-Core CarbonFoam PU 2 R PU
Coastal Enterprises Plus™ PBHT-15 High Density Urethane Foam
Overview of materials for Thermoset Polyurethane Foam, Unreinforced
Covestro Baydur® 660 IBS Polyurethane Structural Foam RIM, Density 40 pcf, MDI-based 2-Component Liquid System
Covestro Bayfit® Low Density Polyurethane Flexible Molded Foam,

PCARBC006 / 190825

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.