MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

AK Steel 13-4 SR® Ferritic Stainless Steel
Categories: Metal; Ferrous Metal; Stainless Steel

Material Notes: AK Steel 13-4 SR Stainless Steel is a ductile weldable ferritic with 13% Cr and 3.75% Al. The high aluminum content results in a base alloy with high electrical resistivity. It is intended for use where electrical energy needs to be dissipated or heat is generated. Good oxidation resistance to 1800°F (982°C) permits applications at elevated temperatures. The alloy’s wet corrosion resistance is comparable to ferritic alloys Type 409 or Type 430.

Information provided by AK Steel.

Key Words: Classified in ASTM B603 Class IV and as UNS K91470
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density  6.95 g/cc
@Temperature 1230 °C
0.251 lb/in³
@Temperature 2250 °F
 7.00 g/cc
@Temperature 1090 °C
0.253 lb/in³
@Temperature 2000 °F
 7.05 g/cc
@Temperature 954 °C
0.255 lb/in³
@Temperature 1750 °F
 7.105 g/cc
@Temperature 816 °C
0.2567 lb/in³
@Temperature 1500 °F
 7.15 g/cc
@Temperature 677 °C
0.258 lb/in³
@Temperature 1250 °F
 7.195 g/cc
@Temperature 538 °C
0.2599 lb/in³
@Temperature 1000 °F
 7.24 g/cc
@Temperature 399 °C
0.262 lb/in³
@Temperature 750 °F
 7.285 g/cc
@Temperature 260 °C
0.2632 lb/in³
@Temperature 500 °F
 7.33 g/cc
@Temperature 121 °C
0.265 lb/in³
@Temperature 250 °F
 7.36 g/cc
@Temperature -17.8 °C
0.266 lb/in³
@Temperature 0.000 °F
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell B 8686
Tensile Strength, Ultimate 558 MPa80900 psiLongitudinal Orientation, True Stress/True Strain
 586 MPa85000 psiTransverse Orientation, True Stress/True Strain
Tensile Strength, Yield  421 MPa
@Strain 0.2 %
61100 psi
@Strain 0.2 %
Longitudinal Orientation, True Stress/True Strain
 448 MPa
@Strain 0.2 %
65000 psi
@Strain 0.2 %
Transverse Orientation, True Stress/True Strain
Elongation at Break 22 %22 %Transverse Orientation, In 2", True Stress/True Strain
 28 %28 %Longitudinal Orientation, In 2", True Stress/True Strain
Rupture Strength  3.70 MPa
@Temperature 871 °C,
Time 3.60e+6 sec
537 psi
@Temperature 1600 °F,
Time 1000 hour
Stress Rupture Strength
 6.30 MPa
@Temperature 871 °C,
Time 360000 sec
914 psi
@Temperature 1600 °F,
Time 100 hour
Stress Rupture Strength
 8.30 MPa
@Temperature 760 °C,
Time 3.60e+6 sec
1200 psi
@Temperature 1400 °F,
Time 1000 hour
Stress Rupture Strength
 15.9 MPa
@Temperature 760 °C,
Time 360000 sec
2310 psi
@Temperature 1400 °F,
Time 100 hour
Stress Rupture Strength
 31.0 MPa
@Temperature 649 °C,
Time 3.60e+6 sec
4500 psi
@Temperature 1200 °F,
Time 1000 hour
Stress Rupture Strength
 46.5 MPa
@Temperature 649 °C,
Time 360000 sec
6740 psi
@Temperature 1200 °F,
Time 100 hour
Stress Rupture Strength
 
Thermal PropertiesMetricEnglishComments
CTE, linear  17.6 µm/m-°C
@Temperature 100 °C
9.79 µin/in-°F
@Temperature 212 °F
 19.1 µm/m-°C
@Temperature 200 °C
10.6 µin/in-°F
@Temperature 392 °F
 20.2 µm/m-°C
@Temperature 300 °C
11.2 µin/in-°F
@Temperature 572 °F
 20.97 µm/m-°C
@Temperature 400 °C
11.65 µin/in-°F
@Temperature 752 °F
 21.69 µm/m-°C
@Temperature 500 °C
12.05 µin/in-°F
@Temperature 932 °F
 22.28 µm/m-°C
@Temperature 600.0 °C
12.38 µin/in-°F
@Temperature 1112 °F
 22.7 µm/m-°C
@Temperature 700.0 °C
12.6 µin/in-°F
@Temperature 1292 °F
 23.38 µm/m-°C
@Temperature 800.0 °C
12.99 µin/in-°F
@Temperature 1472 °F
 24.05 µm/m-°C
@Temperature 900.0 °C
13.36 µin/in-°F
@Temperature 1652 °F
 24.59 µm/m-°C
@Temperature 1000 °C
13.66 µin/in-°F
@Temperature 1832 °F
Thermal Conductivity  13.7 W/m-K
@Temperature 22.8 °C
95.1 BTU-in/hr-ft²-°F
@Temperature 73.0 °F
 14.2 W/m-K
@Temperature 50.0 °C
98.5 BTU-in/hr-ft²-°F
@Temperature 122 °F
 15.0 W/m-K
@Temperature 100 °C
104 BTU-in/hr-ft²-°F
@Temperature 212 °F
 16.6 W/m-K
@Temperature 200 °C
115 BTU-in/hr-ft²-°F
@Temperature 392 °F
 18.2 W/m-K
@Temperature 300 °C
126 BTU-in/hr-ft²-°F
@Temperature 572 °F
 19.8 W/m-K
@Temperature 400 °C
137 BTU-in/hr-ft²-°F
@Temperature 752 °F
 20.5 W/m-K
@Temperature 700.0 °C
142 BTU-in/hr-ft²-°F
@Temperature 1292 °F
 22.8 W/m-K
@Temperature 500 °C
158 BTU-in/hr-ft²-°F
@Temperature 932 °F
 24.0 W/m-K
@Temperature 800.0 °C
167 BTU-in/hr-ft²-°F
@Temperature 1472 °F
 24.8 W/m-K
@Temperature 900.0 °C
172 BTU-in/hr-ft²-°F
@Temperature 1652 °F
 25.1 W/m-K
@Temperature 600.0 °C
174 BTU-in/hr-ft²-°F
@Temperature 1112 °F
 26.2 W/m-K
@Temperature 1000 °C
182 BTU-in/hr-ft²-°F
@Temperature 1832 °F
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 3.75 %3.75 %
Carbon, C 0.025 %0.025 %
Chromium, Cr 13 %13 %
Iron, Fe 82 - 82.375 %82 - 82.375 %Balance
Manganese, Mn 0.30 %0.30 %
Nickel, Ni 0.25 %0.25 %
Phosphorus, P <= 0.045 %<= 0.045 %
Sulfur, S <= 0.030 %<= 0.030 %
Titanium, Ti 0.30 %0.30 %
 
Descriptive Properties
100 Hour Still Air Oxidation Resistance, Weight Gain (mg/cm2)0.191600°F
 0.411800°F
 1.022000°F
 3.232200°F
Cyclic Oxidation Resistance 1550°-1600°F, Weight Change (mg/cm2)0.12100 cycles
 0.13200 cycles
 0.17300 cycles
 0.18400 cycles
 0.18500 cycles
n Value (10% -Ult)0.147Transverse Orientation,True Stress/True Strain
 0.167Longitudinal Orientation, True Stress/True Strain

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
ATI Allegheny Ludlum ALFA-I™ Stainless Steel Type 406
ATI Allegheny Ludlum Stainless Steel Ohmaloy® 40 Resistance Alloy
406 Stainless Steel
Aluminum 6061-T6; 6061-T651
ATI Allegheny Ludlum ALFA-II™ Stainless Steel Type 406

NAKS091a / 140765

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.