MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
BASF Ultraform® N 2310 P Q600 POM
Categories: Polymer; Thermoplastic; Acetal (Polyoxymethylene, POM); Acetal Copolymer, Unreinforced

Material Notes: Product Description: Ultraform® N 2310 P Q600 is a general-purpose injection molding POM grade containing special lubricant. Low friction coefficient giving extremely low wear with otherwise unaltered mechanical properties. Applications: Typical applications include spring elements, clips, gears and other applications requiring low friction and wear.

Availability: North America

Additive: Lubricant

Features: Copolymer; General Purpose; Low Friction; Lubricated; Wear Resistant

Use: Gears; General Purpose; Spring

Agency Ratings: EC 1907/2006 (REACH)

RoSH Compliance: RoSH Compliant

Automotive Specifications: FMVSS 302

Form: Pellets

Processing Method: Injection Molding

Information provided by BASF Corporation

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.40 g/ccISO 1183
Water Absorption 0.20 %Equilibrium, 50% RH; ISO 62
Water Absorption at Saturation 0.80 %ISO 62
Maximum Moisture Content 0.15
Linear Mold Shrinkage, Flow 0.021 cm/cmISO 294-4
Linear Mold Shrinkage, Transverse 0.021 cm/cmISO 294-4
Melt Flow 7.5 g/10 min
@Load 2.16 kg,
Temperature 190 °C
ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Yield 8850 psiISO 527-2
Elongation at Break 30 %Nominal; ISO 527-2
Elongation at Yield 10 %ISO 527-2
Tensile Modulus 377000 psiISO 527-1
Flexural Modulus 339000 psiASTM D790
Izod Impact, Notched 1.00 ft-lb/in
@Temperature -40.0 °C
ASTM D256
 1.20 ft-lb/in
@Temperature 22.8 °C
ASTM D256
Charpy Impact Unnotched 86.0 ft-lb/in²
@Temperature -30.0 °C
ISO 179
 95.0 ft-lb/in²
@Temperature 22.8 °C
ISO 179
Charpy Impact, Notched 2.60 ft-lb/in²ISO 179
Tensile Creep Modulus, 1 hour 276000 psiISO 899-1
Tensile Creep Modulus, 1000 hours 189000 psiISO 899-1
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+14 ohm-cmIEC 60093
Surface Resistance 1.00e+12 ohmIEC 60093
Dielectric Constant 3.8
@Frequency 100 Hz
IEC 60250
 3.8
@Frequency 1e+6 Hz
IEC 60250
Dielectric Strength 1000 V/milIEC 60243-1
Dissipation Factor 0.0010
@Frequency 100 Hz
IEC 60250
 0.0050
@Frequency 1e+6 Hz
IEC 60250
Comparative Tracking Index 600 VSolution A; IEC 60112
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 61.0 µin/in-°FASTM E831
Melting Point 331 °FISO 3146
Deflection Temperature at 0.46 MPa (66 psi) 203 °FUnannealed; ISO 75-2/B
 309 °FUnannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 210 °FUnannealed; ASTM D648
 221 °FUnannealed; ISO 75-2/A
 
Processing PropertiesOriginal ValueComments
Melt Temperature 374 - 446 °F
Mold Temperature 140 - 248 °F
Drying Temperature 176 - 230 °F
Dry Time 2.00 - 4.00 hour
Injection Pressure 508 - 1020 psi

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PBASG2141 / 310834

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.