MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
SABIC PP 6711K Polypropylene Copolymer for Injection Molding  (discontinued **)
Categories: Polymer; Thermoplastic; Polypropylene (PP); Polypropylene, Molded

Material Notes: Product Description: PP 6711K is a controlled rheology grade with narrow molecular weight distribution intended specifically for producing injection molded articles with high clarity, good flow properties & better impact properties than homo PP counterparts. This grade contains advance clarifier & anti-static agent.
PP 6711K has the following features:
  • Consistent processability
  • Good stiffness
  • Excellent clarity
  • Low thickness
  • Easy to flow
  • Better cycle time when compared to normal random grades
  • Less energy consumption

Typical Applications: PP 6711K can be used mainly for clear, thin-wall containers, housewares, caps & closures and lids.

Information provided by SABIC.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.905 g/ccASTM D792
Linear Mold Shrinkage 0.010 - 0.020 cm/cm
Melt Flow 45 g/10 min
@Load 2.16 kg,
Temperature 230 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell R 102ASTM D785
Tensile Strength, Yield 28.0 MPaASTM D638
Elongation at Yield 13 %ASTM D638
Flexural Modulus, 1% Secant 1150 MPaASTM D790A
Izod Impact, Notched 56.0 J/mASTM D256
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 0.46 MPa (66 psi) 75.0 °CASTM D648
Vicat Softening Point 128 °CASTM D1525B
 
Processing PropertiesOriginal ValueComments
Processing Temperature 190 - 230 °CBarrel Temperature
Mold Temperature 30.0 - 40.0 °C

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
SABIC PP 674K Polypropylene Copolymer for Injection Molding
Overview of materials for Polypropylene, Molded
Overview of materials for Acrylic, UV Stabilized, Molded
Alcoa KAMA 7110 Clear Homopolymer Polypropylene (PP)
Lotte Chemical Titan TITANPRO® SM388 Polypropylene random copolymer

PSABICZ877 / 133073

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.