MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Syensqo (Solvay Specialty Polymers) Algoflon® DF 330 F PTFE, Powder
Categories: Polymer; Thermoplastic; Fluoropolymer; Polytetrafluoroethylene (PTFE); Polytetrafluoroethylene (PTFE), Bronze Filled

Material Notes: Algoflon® DF 330 F is a white fine coagulated powder and is produced without any intentional use or addition of PFOA. It is designed for paste extrusion in low reduction (RR) range. It is recommended for extrusion of large tubes diameters followed by continuous or batch sintering. It can be used also for manufacture of tapes for wrapping and as additive in plastics for improving their anti-dripping behavior.

Algoflon® DF 330 F exhibits excellent green strength and wrapping behavior and low permeability.

Main features of Algoflon® DF 330 F include:
- Excellent green strength
- Excellent wrapping properties
- Good weldability
- Low permeability
- Optimum electrical properties
- Good anti-dripping effect

Applications: Aerospace Applications; Automotive Applications; Electrical/Electronic Applications; Industrial Applications; Tubing; Wire & Cable Applications

Features: Chemical Resistant; Good Processing Stability; Good Thermal Stability; Low Friction

Processing
- Algoflon® DF 330 F is processed according to methods conventionally used for paste extrusion. Initially the powder is mixed with a lubricant to produce a paste. This is then compacted into a preform and extruded through a finishing die using a ram extruder.
- In the production of electrical tapes, further processing as calendering and removal of lubricant can then be carried out to make the final product. For tubing, the lubricant is removed using heat and then the dried extrudate is sintered and cooled to attain the finished tube with specific properties.
- Regarding anti-drip effect, Algoflon DF 330 F content in the range 0.5 - 1 % by weight should be enough to enhance anti-drip property. It is recommended sieving DF 330 F before mixing with others ingredients and feeding in plastics like PC or ABS during extrusion.

Storage and Handling
- Algoflon® PTFE fine coagulated powders must be stored and handled carefully to avoid excessive shearing and particle fibrillation. Fibrillation is irreversible and damaged particles can appear as defects in manufactured articles.
- PTFE fine coagulated powders must be handled below 19°C because above this temperature the powders are softer and can be more easily laminated. It is recommended sieving of powders below 19°C before mixing with others ingredients. Strong vibrations and shocks must be avoided as much as possible for prevent lumps formation.
- Storage and transportation should be carried out in the range 5 - 19°C. Moreover, the powders must be stored in a dry room because the absorption of moisture could negatively affect its processing.
- Storage and handling facilities should be clean since even very small foreign particles can cause defects in finished products. Keep resin drums closed and clean. Good housekeeping and careful handling are essential.

Safety and Toxicology
- Before using Algoflon® PTFE fine coagulated powders consult the product Material Safety Data Sheet and follow all label directions and handling precautions.
- As with all PTFE materials, handling and processing should only be carried out in well ventilated areas. Vapor extractor units should be installed above processing equipment. Fumes must not be inhaled and eye and skin contact ought to be avoided. In case of skin contacts wash with soap and water. In case of eye contact flush with water immediately and seek medical help. Do not smoke in areas contaminated with powder, vapor or fumes.

Information provided by Solvay Specialty Polymers.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 2.14 g/cc2.14 g/ccASTM D792
Bulk Density 0.475 g/cc0.0172 lb/in³ASTM D4894
Particle Size 600 µm600 µmAverage
Viscosity 1.00e+11 cP1.00e+11 cP
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength 35.0 MPa5080 psiASTM D4894
 
Descriptive Properties
AvailabilityAsia Pacific
 Europe
 North America
ColorWhite
FormsPowder

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PSOL8Y4024 / 279824

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.