MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
E-Polymers SEPAZ® N1040 Nanoclay 4% High Flow Nano Composite Resin
Categories: Polymer; Thermoplastic

Material Notes: Nanocomposite: SEPAZ Nano PA6 nanocomposites have been prepared successfully in commercial scale through 'in situ' polymerization or melt extrusion. The performance properties of nanocomposities provide great flexibility in materials design. Nanocomposites have been formulated into various resin systems to deliver desired properties: from rheology control to fire retardation. It shows low specific gravity, gas permeability and high heat resistance, rigidity, dimension stability used for underhood and fuel line parts in automotive industry and for packaging film in food industry.

Information Provided by E-Polymers Co., Ltd.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.15 g/ccASTM D792
Water Absorption 0.90 %
@Time 86400 sec
Linear Mold Shrinkage 0.0060 cm/cm
Linear Mold Shrinkage, Transverse 0.0080 cm/cm
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength 105.0 MPaASTM D638
Elongation at Break 1.4 %ASTM D638
Flexural Strength 166.28 MPaASTM D790
Flexural Modulus 4591 MPaASTM D790
Izod Impact, Notched 3.20 kg-cm/cmASTM D256
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 1.8 MPa (264 psi) 150 °CASTM D648
Flammability, UL94 HB
 
Processing PropertiesOriginal ValueComments
Melt Temperature 221 °C
Mold Temperature 40.0 - 60.0 °C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Ravago Manufacturing Americas Hylon® N1040MGHL Nylon 6/6 (Cond)
Eurotec® Tecomid® NB40 GB30 NL PA6, 30% glass bead reinforced, natural
E-Polymers SEPAZ® N3040HR Nanoclay 3% Dimensional stability, Super Toughness Nano Composite Resin
Oxford Polymers Stranox PA6/30% Glass Fiber Reinforced Nylon 6
NCMT NanoPAC™ S206 High Performance Polypropylene Nanocomposite

PEPOLZ096 / 103593

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.