MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

USP Class VI Adhesives
USP Class VI Approved Adhesives for Medical Device Applications
Master Bond’s biocompatible adhesives are designed to meet the needs of medical device manufacturers. Compounds withstand various types of sterilization methods.

(Viewing data as-entered. Click here to return)
Avient Versaflex™ CL2242 Thermoplastic Elastomer (TPE)
Categories: Polymer; Thermoplastic; Elastomer, TPE

Material Notes: Versaflex™ CL2242 is an easy processing compound designed for use in injection molding applications where FDA compliance, clarity and enhanced heat resistance are required. - Excellent Clarity - Overmold Adhesion to Polypropylene - Superior Colorability - Very Good Heat and Boil Resistance

Color concentrates based on polypropylene (PP), ethylene vinyl acetate (EVA), or polyethylene (PE) are most suitable for coloring Versaflex™ CL2242. Improved color dispersion can be achieved by using higher melt flow concentrates (with a melt flow from 25-40 g/10 min). Typical loadings for color concentrates are 1% to 5% by weight. Liquid color can be used, but mineral oil based carriers may have a significant effect on the final hardness value. Concentrates based on PVC should not be used. A high color match consistency can be obtained by the use of precolored compounds available from GLS. The final determination of color concentrate suitability should be determined by customer trials. Purge thoroughly before and after use of this product with a low flow (0.5 - 2.5 MFR) polyethylene (PE) or polypropylene (PP). Regrind levels up to 20% can be used with Versaflex™ CL2242 with minimal property loss, provided that the regrind is free of contamination. To minimize losses during molding, the melt temperature should remain as low as possible. The final determination of regrind effectiveness should be determined by the customer. Versaflex™ CL2242 has excellent melt stability. Maximum residence times may vary, depending on the size of the barrel. Generally, the barrel should be emptied if it is idle for periods of 8 - 10 minutes or longer. Drying is not Required Injection Speed: 0.5 to 2 in/sec 1st Stage - Boost Pressure: 100 to 800 psi 2nd Stage - Hold Pressure: 30% of Boost Hold Time (Thick Part): 4 to 10 sec Hold Time (Thin Part): 1 to 3 sec

Information provided by PolyOne

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 0.888 g/ccASTM D792
Viscosity 9700 cP
@Shear Rate 11200 1/s,
Temperature 200 °C
ASTM D3835
Linear Mold Shrinkage, Flow 0.0070 - 0.011 cm/cmASTM D955
Melt Flow 26 g/10 min
@Load 2.16 kg,
Temperature 190 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 4310 sec; ASTM D2240
Tensile Strength at Break 5.04 MPa
@Temperature 23.0 °C
Die C2 hr; ASTM D412
Tensile Stress at Strain 1.05 MPa
@Strain 100 %,
Temperature 23.0 °C
Die C2 hr; ASTM D412
 2.03 MPa
@Strain 300 %,
Temperature 23.0 °C
Die C2 hr; ASTM D412
Elongation at Break 780 %
@Temperature 23.0 °C
Die C2 hr; ASTM D412
Flexural Modulus 7.21 MPaASTM D790
Tear Strength 21.7 kN/mASTM D624
Compression Set 23 %
@Temperature 23.0 °C,
Time 79200 sec
ASTM D395B
 
Processing PropertiesOriginal ValueComments
Rear Barrel Temperature 171 - 188 °C
Middle Barrel Temperature 193 - 221 °C
Front Barrel Temperature 193 - 227 °C
Nozzle Temperature 210 - 227 °C
Melt Temperature 210 - 221 °C
Mold Temperature 12.8 - 37.8 °C
Back Pressure 0.000 - 0.552 MPa
Screw Speed 25 - 75 rpm
 
Compliance PropertiesOriginal ValueComments
FDA YesUnspecified Rating
USP Class VI Yes
 
Descriptive Properties
Agency RatingsISO 10993 Part 4
 ISO 10993 Part 5
AppearanceClear/Transparent
FeaturesGood Colorability
 Good Moldability
 Good Processability
 Good Processing Stability
 High Clarity
FormsPellets
Generic MaterialTPE
Generic NameThermoplastic Elastomer (TPE)
Processing MethodInjection Molding
Regional AvailabilityAfrica & Middle East
 Asia Pacific
 Europe
 North America
 South America
RoHS ComplianceRoHS Compliant
Suggested Max Regrind20%
UsesMedical/Healthcare Applications
 Overmolding
 Pacifiers
 Personal Care
 Transparent or Translucent Parts
 Transparent Parts

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Avient Versaflex™ CL30 Thermoplastic Elastomer (TPE)
Avient Versaflex™ OM 1040X-1 Thermoplastic Elastomer (TPE)
Advanced Elastomer Systems Santoprene® 181-55 Thermoplastic Rubber
Avient Versaflex™ CL2000X Thermoplastic Elastomer (TPE)
Avient Versaflex™ CL2250 Thermoplastic Elastomer (TPE)

PH0POL0843 / 145412

USP Class VI adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.