MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Chemically Resistant adhesives

ITW Epocast 36P Epoxy Chocking Compound
Categories: Polymer; Thermoset; Epoxy

Material Notes: EPOCAST 36-P is a trowelable thixotropic 2-component epoxy paste especially developed for installation of LPG/LNG tanks and other containment systems. EPOCAST 36-P is a further development of EPOCAST 36®. EPOCAST 36-P can be extremely loaded. It has good adhesive properties, even at very low temperatures. EPOCAST 36-P has been approved by all major Classification Societies for temperatures from +80°C to -165°C.

Uses: Mounting of LPG/LNG tanks, chemical tanks and other containment systems, sliding doors, anchor plates etc. Positioning of laminated wood blocks to tank surfaces and tank saddles, eliminating all precision fitting.

Information provided by ITW Performance Polymers.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Mechanical PropertiesMetricEnglishComments
Hardness, Barcol >= 30>= 30
Modulus of Elasticity 0.0860 GPa12.5 ksiat room ambient temperature
 7.12 GPa
@Temperature -110 °C
1030 ksi
@Temperature -166 °F
 9.99 GPa
@Temperature -195 °C
1450 ksi
@Temperature -319 °F
Compressive Strength  >= 86.2 MPa
@Temperature 23.0 °C
>= 12500 psi
@Temperature 73.4 °F
 197 MPa
@Temperature -110 °C
28600 psi
@Temperature -166 °F
 215 MPa
@Strain 3.11 %,
Temperature -195 °C
31200 psi
@Strain 3.11 %,
Temperature -319 °F
Shear Strength  1.80 MPa
@Temperature -165 °C
261 psi
@Temperature -265 °F
 12.1 MPa
@Temperature -110 °C
1750 psi
@Temperature -166 °F
 
Thermal PropertiesMetricEnglishComments
Specific Heat Capacity 1.354 J/g-°C0.3236 BTU/lb-°F
Thermal Conductivity 0.684 W/m-K4.75 BTU-in/hr-ft²-°F
Minimum Service Temperature, Air 13.0 °C55.4 °F
 
Processing PropertiesMetricEnglishComments
Cure Time 240 - 360 min4.00 - 6.00 hourStarting to cure
 4320 min72.0 hourReady to take loading
 10100 min168 hourFully cured
Shelf Life 18.0 Month18.0 Month

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Resinlab® SEC1222 Silver Filled Epoxy Adhesive
Tipco Tipwood® 50 EX 50EX
Resinlab® SEC1233 Silver Filled Epoxy Adhesive
Oceanchem Group 2,2-Dibromo-3-nitrilopropionamide (DBNPA)
Master Bond EP21TDC-4ND Two component, highly flexibilized epoxy for bonding, sealing and coating

PITWE9043 / 239553

Chemically Resistant adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.