MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
DuPont™ Dartek® B-602 Nylon 6,6 Barrier Film, 38 µm Thickness, PVDC Coated  (discontinued **)
Categories: Polymer; Film; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, Film

Material Notes: Data provided by DuPont Packaging Polymers.

A strong, transparent nylon 6,6 film which has a PVDC coating applied to one side for enhanced barrier to oxygen, moisture, grease and odor. It is specially formulated for use in high humidity applications. Can be printed, laminated, or extrusion coated. In converter combinations, it can be used for any packaging or industrial end use requiring high barrier properties. It can be easily thermoformed for assorted shapes and products such as meats and cheeses.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.15 g/cc
Moisture Vapor Transmission 0.340 cc-mm/m²-24hr-atm
@Temperature 38.0 °C
90% RH; ASTM F-372
Water Vapor Transmission 9.00 g/m²/day
@Temperature 38.0 °C
90% RH; ASTM F-372
Oxygen Transmission 0.290 cc-mm/m²-24hr-atmor 7.7 cc/m²-24hr-atm for the film at 23°C, 0% RH. ASTM D1434-66
Thickness 38.0 mil
 
Mechanical PropertiesOriginal ValueComments
Film Elongation at Break, MD 300 %ASTM D882-64T
Film Elongation at Break, TD 300 %ASTM D882-64T
Secant Modulus, MD 0.690 GPaASTM D882
Secant Modulus, TD 0.690 GPaASTM D882
Coefficient of Friction, Dynamic 0.45film to coating; ASTM D1894-63
Elmendorf Tear Strength, MD 1.40 g/micronASTM D1922-67
Elmendorf Tear Strength, TD 1.20 g/micronASTM D1922-67
Dart Drop Test 600 gImpact Strength, ASTM D1709-62T
Film Tensile Strength at Break, MD 70.0 MPaASTM D882
Film Tensile Strength at Break, TD 70.0 MPaASTM D882
 
Optical PropertiesOriginal ValueComments
Haze 1.5 %
Gloss 150 %
Transmission, Visible 90 %transparent; thickness not quantified

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Overview of materials for Polyvinyl Dichloride (PVDC)
DuPont™ Dartek® B-601 Nylon 6,6 Barrier Film, 25 µm Thickness
DuPont™ Dartek® SF-502 Nylon 6,6 Super Formable Film, 76 µm Thickness
Teknor Apex Chemlon® 133 GVH Nylon 66, 30% Glass Fiber Reinforced
UBE UPIMOL® SA201 Heat-Resistant Polyimide Shape

PDU744 / 33163

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.