MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

Thermal Ceramics Kaowool 3000M High Temperature Board
Categories: Ceramic; Oxide; Aluminum Oxide

Material Notes: Kaowool 3000M is processed using a blend of high purity ceramic fibers and high temperature mullite fibers and alumina mix. Kaowool 3000M has excellent temperature stability, shrinkage and mechanical strengths after firing for temperatures up to 2900°F (1593°C).

Applications:

  • Appliance and heat processing
  • Backup insulation to dense refractories
  • Bullnose tiles
  • Burner blocks
  • Combustion chamber construction
  • Expansion joint material
  • Flue and chimney linings
  • Furnace components
  • Furnace door linings
  • Furnace, kiln, and oven hot face linings
  • Glass regenerator insulation
  • Heat shields
  • High temperature gaskets and seals
  • Peep door frames and plugs
  • Shapes in ammonia reformers
  • Information provided by Thermal Ceramics

    Data has not been recently verified. Please contact manufacturer for current information.

    Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
     
    Physical PropertiesMetricEnglishComments
    Density 0.224 g/cc0.00809 lb/in³
    Loss On Ignition 7.0 - 9.0 %7.0 - 9.0 %
     
    Mechanical PropertiesMetricEnglishComments
    Modulus of Rupture 0.000862 GPa0.125 ksi
    Compressive Yield Strength 0.210 MPa30.5 psiat 5% deformation
     0.240 MPa34.8 psiat 10% deformation
     
    Thermal PropertiesMetricEnglishComments
    Thermal Conductivity  0.0692 W/m-K
    @Temperature 260 °C
    0.480 BTU-in/hr-ft²-°F
    @Temperature 500 °F
     0.0951 W/m-K
    @Temperature 538 °C
    0.660 BTU-in/hr-ft²-°F
    @Temperature 1000 °F
     0.140 W/m-K
    @Temperature 816 °C
    0.970 BTU-in/hr-ft²-°F
    @Temperature 1500 °F
     0.205 W/m-K
    @Temperature 1090 °C
    1.42 BTU-in/hr-ft²-°F
    @Temperature 2000 °F
     0.297 W/m-K
    @Temperature 1370 °C
    2.06 BTU-in/hr-ft²-°F
    @Temperature 2500 °F
    Melting Point 1820 °C3300 °F
    Maximum Service Temperature, Air 1590 °C2900 °F
    Shrinkage  0.10 %
    @Temperature 982 °C,
    Time 86400 sec
    0.10 %
    @Temperature 1800 °F,
    Time 24.0 hour
     0.10 %
    @Temperature 1090 °C,
    Time 86400 sec
    0.10 %
    @Temperature 2000 °F,
    Time 24.0 hour
     0.20 %
    @Temperature 1540 °C,
    Time 86400 sec
    0.20 %
    @Temperature 2800 °F,
    Time 24.0 hour
     0.30 %
    @Temperature 816 °C,
    Time 86400 sec
    0.30 %
    @Temperature 1500 °F,
    Time 24.0 hour
     0.40 %
    @Temperature 1430 °C,
    Time 86400 sec
    0.40 %
    @Temperature 2600 °F,
    Time 24.0 hour
     0.50 %
    @Temperature 1320 °C,
    Time 86400 sec
    0.50 %
    @Temperature 2400 °F,
    Time 24.0 hour
     0.90 %
    @Temperature 1590 °C,
    Time 86400 sec
    0.90 %
    @Temperature 2900 °F,
    Time 24.0 hour
     
    Component Elements PropertiesMetricEnglishComments
    Al2O3 71 %71 %
    Other 7.0 - 9.0 %7.0 - 9.0 %
    SiO2 29 %29 %

    Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

    Users viewing this material also viewed the following:
    Zircar Zirconia BusterF-10 Alumina Bulk Fiber Insulation
    Thermal Ceramics 2800 RPC Shapes
    Poco Graphite AXF-5QC Specialty Graphite, Copper Impregnated
    Momentive Performance Materials HPC Boron Nitride (BN)/TiO2 Water Based Coating
    Momentive Performance Materials FPD Boron Nitride (BN) Coating

    CTHERM183 / 2503

    Free Trade Publications, Click Here!
    Free Trade Publications, Click Here!

    Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

    The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.