MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Chi Mei Wonderlite® PC-681U PC
Categories: Polymer; Thermoplastic; Polycarbonate (PC); Polycarbonate, Molded

Material Notes: Product Description: 1.5mm V-0, Opaque, UV Stabilized, UL 746C f1, Low temperature

Availability: Africa & Middle East; Europe; Asia Pacific; Latin America; North America

Additive: Flame Retardant; UV Stabilizer

Features: Flame Retardant; Low Temperature Resistant; UV Stabilized

RoSH Compliance: RoSH Compliant

Appearance: Opaque

Resin ID (ISO 1043): >PC<

Information provided by Chi Mei Corporation

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.20 g/cc0.0434 lb/in³ISO 1183
Linear Mold Shrinkage 0.0040 - 0.0060 cm/cm0.0040 - 0.0060 in/inISO 294-4
Melt Flow 10 g/10 min
@Load 2.16 kg,
Temperature 260 °C
10 g/10 min
@Load 4.76 lb,
Temperature 500 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 65.0 MPa9430 psiISO 527-2/50
Tensile Strength, Yield 60.0 MPa8700 psiISO 527-2/50
Elongation at Break 120 %120 %ISO 527-2/50
Flexural Strength 90.3 MPa13100 psi0.079 in/min; ISO 178
Flexural Modulus 2.30 GPa334 ksi0.079 in/min; ISO 178
Izod Impact, Notched (ISO)  44.1 kJ/m²
@Temperature -30.0 °C
21.0 ft-lb/in²
@Temperature -22.0 °F
ISO 180/1A
 60.9 kJ/m²
@Temperature 22.8 °C
29.0 ft-lb/in²
@Temperature 73.0 °F
ISO 180/1A
Charpy Impact, Notched  4.41 J/cm²
@Temperature -30.0 °C
21.0 ft-lb/in²
@Temperature -22.0 °F
ISO 179
 6.09 J/cm²
@Temperature 22.8 °C
29.0 ft-lb/in²
@Temperature 73.0 °F
ISO 179
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 6.30e+15 ohm-cm6.30e+15 ohm-cmIEC 60093
Surface Resistance 6.90e+13 ohm6.90e+13 ohmIEC 60093
Dielectric Constant 3.0
@Frequency 1e+6 Hz
3.0
@Frequency 1e+6 Hz
IEC 60250
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 64.8 µm/m-°C36.0 µin/in-°FISO 11359-2
Deflection Temperature at 1.8 MPa (264 psi) 125 °C257 °FUnannealed; ISO 75-2/A
 140 °C284 °FAnnealed; ISO 75-2/A
Vicat Softening Point 145 °C293 °FISO 306/B50
 150 °C302 °FISO 306/A50
Flammability, UL94  V-0
@Thickness 1.52 mm
V-0
@Thickness 0.0600 in
 5VA
@Thickness 3.05 mm
5VA
@Thickness 0.120 in

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PCHJ370 / 311063

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.