MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Envalior Durethan® AKV 35 000000 Nylon 66 (PA66), 35% Glass Fiber Reinforced, Conditioned
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, 40% Glass Fiber Filled

Material Notes: PA 66, 35% glass fibers, injection molding

Former Lanxess product line is now with Envalior.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.41 g/ccISO 1183
Moisture Absorption at Equilibrium 1.8 %50% RH; ISO 62
Water Absorption at Saturation 5.0 %ISO 62
Linear Mold Shrinkage, Flow 0.0032 cm/cm150x105x3; 300 °C / MT 80 °C; 400 bar; ISO 294-4
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 135 MPa5 mm/min; ISO 527-1,-2
Elongation at Break 5.0 %5 mm/min; ISO 527-1,-2
Tensile Modulus 7500 MPa1 mm/min; ISO 527-1,-2
Flexural Strength 220 MPa2 mm/min; ISO 178-A
Flexural Yield Strength 170 MPa
@Strain 3.5 %
2 mm/min; ISO 178-A
Flexural Modulus 7000 MPa2 mm/min; ISO 178-A
Flexural Strain at Break 6.0 %2 mm/min; ISO 178-A
Izod Impact, Notched (ISO) <= 10.0 kJ/m²
@Temperature 23.0 °C
ISO 180-1A
 <= 10.0 kJ/m²
@Temperature -30.0 °C
ISO 180-1A
Charpy Impact Unnotched 75.0 kJ/m²
@Temperature -30.0 °C
ISO 179-1eU
 95.0 kJ/m²
@Temperature 23.0 °C
ISO 179-1eU
Charpy Impact, Notched 10.0 kJ/m²
@Temperature -30.0 °C
ISO 179 1eA
 20.0 kJ/m²
@Temperature 23.0 °C
ISO 179 1eA
Tensile Creep Modulus, 1 hour 7000 MPaISO 899-1
Tensile Creep Modulus, 1000 hours 5800 MPaISO 899-1
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+10 ohm-cmIEC 60093
Surface Resistance 1.00e+12 ohmIEC 60093
Dielectric Constant 4.0
@Frequency 1e+6 Hz
IEC 60250
 10
@Frequency 100 Hz
IEC 60250
Dielectric Strength 35.0 kV/mm
@Thickness 1.00 mm
IEC 60243-1
 
Thermal PropertiesOriginal ValueComments
Melting Point 263 °C10°C/min; ISO 11357-1,-3
 
Processing PropertiesOriginal ValueComments
Melt Temperature 290 °Cinjection molding; ISO 294

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Envalior Durethan® AKV 35 H3.0 000000 Nylon 66 (PA66), 35% Glass Fiber Reinforced, Dry
Envalior Durethan® AKV 35 000000 Nylon 66 (PA66), 35% Glass Fiber Reinforced, Dry
Envalior Durethan® AKV 35 HR H2.0 901510 Nylon 66 (PA66), 35% Glass Fiber Reinforced, Dry
Envalior Durethan® AKV 35 HR H2.0 901510 Nylon 66 (PA66), 35% Glass Fiber Reinforced, Conditioned
Envalior Durethan® AKV 35 H3.0 000000 Nylon 66 (PA66), 35% Glass Fiber Reinforced, Conditioned

PLANW9233 / 208030

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.