MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Morgan Advanced Ceramics Hicast 90 Thermal Ceramic
Categories: Ceramic; Oxide

Material Notes: Material method of installation is vibratory cast.

Information provided by Morgan Advanced Materials

Key Words: Thermal Ceramic
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 2.851 - 3.027 g/cc
@Temperature 816 °C
0.1030 - 0.1094 lb/in³
@Temperature 1500 °F
fired; ASTM C-134
Deformation 0.60 %
@Pressure 0.172 MPa
0.60 %
@Pressure 25.0 psi
under hot load, dried 24hrs @ 104°C; ASTM C16
 
Mechanical PropertiesMetricEnglishComments
Modulus of Rupture  0.0100 - 0.0140 GPa
@Temperature 816 °C,
Time 18000 sec
1.45 - 2.03 ksi
@Temperature 1500 °F,
Time 5.00 hour
dried; ASTM C 133
 0.0110 - 0.0170 GPa
@Temperature 104 °C,
Time 86400 sec
1.60 - 2.47 ksi
@Temperature 219 °F,
Time 24.0 hour
dried; ASTM C 133
Compressive Strength  69.0 - 97.0 MPa
@Temperature 104 °C,
Time 86400 sec
10000 - 14100 psi
@Temperature 219 °F,
Time 24.0 hour
Cold Crushing Strength, dried; ASTM C133
 76.0 - 124 MPa
@Temperature 816 °C,
Time 18000 sec
11000 - 18000 psi
@Temperature 1500 °F,
Time 5.00 hour
Cold Crushing Strength, dried; ASTM C133
 90.0 - 138 MPa
@Temperature 1671 °C,
Time 18000 sec
13100 - 20000 psi
@Temperature 3040 °F,
Time 5.00 hour
Cold Crushing Strength, fired; ASTM C133
Abrasion 5.0 - 8.0
@Temperature 816 °C
5.0 - 8.0
@Temperature 1500 °F
cm3, loss, fired at 815°C; ASTM C704
 
Thermal PropertiesMetricEnglishComments
Thermal Conductivity  1.72 W/m-K
@Temperature 815 °C
11.9 BTU-in/hr-ft²-°F
@Temperature 1500 °F
ASTM C201
 1.74 W/m-K
@Temperature 1093 °C
12.1 BTU-in/hr-ft²-°F
@Temperature 1999 °F
ASTM C201
 3.32 W/m-K
@Temperature 538 °C
23.0 BTU-in/hr-ft²-°F
@Temperature 1000 °F
ASTM C201
 4.08 W/m-K
@Temperature 260 °C
28.3 BTU-in/hr-ft²-°F
@Temperature 500 °F
ASTM C201
Maximum Service Temperature, Air <= 1671 °C<= 3040 °F
Shrinkage  0.00 - 0.20 %
@Treatment Temp. 104 °C,
Time 86400 sec
0.00 - 0.20 %
@Treatment Temp. 219 °F,
Time 24.0 hour
dried; ASTM C 113
 0.10 - 0.30 %
@Treatment Temp. 816 °C,
Time 18000 sec
0.10 - 0.30 %
@Treatment Temp. 1500 °F,
Time 5.00 hour
fired; ASTM C 113
 0.50 - 1.5 %
@Treatment Temp. 1671 °C,
Time 18000 sec
0.50 - 1.5 %
@Treatment Temp. 3040 °F,
Time 5.00 hour
fired; ASTM C 113
 
Processing PropertiesMetricEnglishComments
Moisture Content 4.0 - 4.5 %4.0 - 4.5 %recommended, casting by vibrating
Shelf Life 6.00 Month6.00 Month
 
Component Elements PropertiesMetricEnglishComments
Al2O3 92 %92 %
CaO 1.2 %1.2 %
Fe2O3 0.10 %0.10 %
NaO2 0.40 %0.40 %as Na2O
SiO2 6.2 %6.2 %
 
Descriptive Properties
Placement, average (kg)83to place 1m3

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

CMORF6064 / 202848

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.