Physical Properties | Original Value | Comments |
---|
Specific Gravity | 1.53 g/cc |
Density | 1.53 g/cc |
Filler Content | 30 % |
Water Absorption | 0.090 % @Time 86400 sec |
Moisture Absorption at Equilibrium | 0.080 % |
Linear Mold Shrinkage, Flow | 0.0030 - 0.0070 cm/cm |
| 0.0030 - 0.0050 cm/cm @Thickness 1.50 - 3.20 mm |
| 0.0030 - 0.0080 cm/cm @Thickness 3.20 mm |
| 0.0050 - 0.0080 cm/cm @Thickness 3.20 - 4.60 mm |
Linear Mold Shrinkage, Transverse | 0.0050 - 0.010 cm/cm |
| 0.0040 - 0.0060 cm/cm @Thickness 1.50 - 3.20 mm |
| 0.0060 - 0.0090 cm/cm @Thickness 3.20 - 4.60 mm |
| 0.0050 - 0.010 cm/cm @Thickness 3.20 mm |
Melt Flow | 13 g/10 min @Load 2.16 kg, Temperature 250 °C |
| 17 g/10 min @Load 2.16 kg, Temperature 250 °C |
|
Mechanical Properties | Original Value | Comments |
---|
Hardness, Rockwell R | 118 |
| 118 |
Hardness, H358/30 | 122 MPa |
Tensile Strength at Break | 120 MPa |
| 125 MPa |
Tensile Strength, Yield | 120 MPa |
| 125 MPa |
Elongation at Break | 2.0 % |
| 2.7 % |
Elongation at Yield | 2.0 % |
| 2.7 % |
Tensile Modulus | 9300 MPa |
| 9300 MPa |
Flexural Strength | 189 MPa |
Flexural Yield Strength | 195 MPa |
| 195 MPa |
Flexural Modulus | 7580 MPa |
| 8500 MPa |
Izod Impact, Notched | 80.0 J/m @Temperature -30.0 °C |
| 85.0 J/m @Temperature 23.0 °C |
Izod Impact, Unnotched | 8.01 J/cm @Temperature 23.0 °C |
Izod Impact, Notched (ISO) | 7.00 kJ/m² @Temperature -30.0 °C |
| 8.00 kJ/m² @Temperature 23.0 °C |
Izod Impact, Unnotched (ISO) | 45.0 kJ/m² @Temperature 23.0 °C |
| 45.0 kJ/m² @Temperature -30.0 °C |
Charpy Impact Unnotched | 45.0 kJ/m² @Temperature 23.0 °C |
| 45.0 kJ/m² @Temperature -30.0 °C |
Charpy Impact, Notched | 5.00 kJ/m² @Temperature 23.0 °C |
| 5.00 kJ/m² @Temperature -30.0 °C |
Instrumented Impact Total Energy | 8.00 J @Temperature 23.0 °C |
Taber Abrasion, mg/1000 Cycles | 19 @Load 1.00 kg |
|
Electrical Properties | Original Value | Comments |
---|
Volume Resistivity | >= 1.00e+15 ohm-cm |
| >= 3.20e+16 ohm-cm |
Surface Resistance | >= 1.00e+15 ohm |
Dielectric Constant | 3.1 @Frequency 1e+6 Hz |
| 3.1 @Frequency 50.0 - 60.0 Hz |
| 3.7 @Frequency 1e+6 Hz |
| 3.8 @Frequency 100 Hz |
Dielectric Strength | 16.0 kV/mm @Thickness 3.20 mm |
| 18.7 kV/mm @Thickness 3.20 mm |
| 19.0 kV/mm @Thickness 1.00 mm |
| 24.0 kV/mm @Thickness 1.60 mm |
| 24.8 kV/mm @Thickness 1.60 mm |
| 28.0 kV/mm @Thickness 0.800 mm |
Dissipation Factor | 0.0010 @Frequency 50.0 - 60.0 Hz |
| 0.0010 @Frequency 100 Hz |
| 0.0020 @Frequency 100 Hz |
| 0.010 @Frequency 1e+6 Hz |
| 0.020 @Frequency 1e+6 Hz |
Arc Resistance | 120 - 180 sec |
Comparative Tracking Index | 300 V |
| >= 600 V |
High Voltage Arc-Tracking Rate, HVTR | 10.0 - 25.4 mm/min |
|
Thermal Properties | Original Value | Comments |
---|
CTE, linear, Parallel to Flow | 25.2 µm/m-°C @Temperature -40.0 - 40.0 °C |
| 25.2 µm/m-°C @Temperature 60.0 - 138 °C |
| 25.2 µm/m-°C @Temperature -40.0 - 40.0 °C |
CTE, linear, Transverse to Flow | 120 µm/m-°C @Temperature -40.0 - 40.0 °C |
| 120 µm/m-°C @Temperature -40.0 - 40.0 °C |
Thermal Conductivity | 0.190 W/m-K |
Deflection Temperature at 0.46 MPa (66 psi) | 217 °C |
| 215 °C @Thickness 6.40 mm |
| 220 °C @Thickness 3.20 mm |
Deflection Temperature at 1.8 MPa (264 psi) | 204 °C |
| 203 °C @Thickness 3.20 mm |
| 207 °C @Thickness 6.40 mm |
Vicat Softening Point | 215 °C |
| 215 °C |
| 215 °C |
| 223 °C |
UL RTI, Electrical | 140 °C |
UL RTI, Mechanical with Impact | 140 °C |
UL RTI, Mechanical without Impact | 140 °C |
Flammability, UL94 | HB @Thickness 0.840 mm |
Oxygen Index | 19 % |
Glow Wire Flammability Index | 750 °C @Thickness 1.00 mm |
|
Descriptive Properties |
---|
Ball Pressure Test, 125°C +/- 2°C | PASSES |
Some of the values displayed above may have been converted from their original units and/or rounded in order to
display the information in a consistent format. Users requiring more precise data for scientific or engineering
calculations can click on the property value to see the original value as well as raw conversions to equivalent units.
We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding
error. We also ask that you refer to MatWeb's
terms of use regarding this information.
Click here to go back to viewing the property data in MatWeb's normal format.