MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
Silver-bearing tough pitch Copper, UNS C11600, H04 Temper, Rod
Categories: Metal; Nonferrous Metal; Copper Alloy

Material Notes: Temper: Hard

Fabrication Properties: Excellent Suitability – Soldering, Capacity for Being Cold Worked, Capacity for Being Hot Formed; Good Suitability – Brazing, Butt Weld; Fair Suitability – Gas Shielded Arc Welding

Common Fabrication Processes: Blanking, Coining, Coppersmithing, Drawing, Etching, Forming and Bending, Heading and Upsetting, Hot Forging and Pressing, Piercing and Punching, Roll Threading and Knurling, Shearing, Spinning, Squeezing and Swaging, Stamping

Typical uses: Gaskets; Radiators; Bus Bars; Commutator Bars and Segments; Conductivity Wire; Contacts; Fuse Clips; Generator Coils; Radio Parts; Switches; Terminals; Windings; Chemical Process Equipment; Clad Metals; Printed Circuit Foil; Printing Rolls

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.322 lb/in³
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell B 45
@Thickness 50.8 mm
 47
@Thickness 25.4 mm
 60
@Thickness 6.35 mm
Hardness, Rockwell F 85
@Thickness 50.8 mm
 87
@Thickness 25.4 mm
 94
@Thickness 6.35 mm
Tensile Strength 45.0 ksi
@Thickness 50.8 mm
 48.0 ksi
@Thickness 25.4 mm
 55.0 ksi
@Thickness 6.35 mm
Tensile Strength, Yield 40.0 ksi
@Thickness 50.8 mm
0.5% Ext
 44.0 ksi
@Thickness 25.4 mm
0.5% Ext
 50.0 ksi
@Thickness 6.35 mm
0.5% Ext
Elongation at Break 10 %
@Thickness 6.35 mm
 16 %
@Thickness 25.4 mm
 20 %
@Thickness 50.8 mm
Tensile Modulus 17000 ksi
Modulus of Rigidity 6400 ksi
Poissons Ratio 0.33Calculated
Machinability 20 %
Forgeability 65 %
Shear Strength 26.0 ksi
@Thickness 50.8 mm
 27.0 ksi
@Thickness 25.4 mm
 29.0 ksi
@Thickness 6.35 mm
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.00000172 ohm-cm100% IACS
 
Thermal PropertiesOriginal ValueComments
CTE, linear 9.80 µin/in-°F
@Temperature 20.0 - 300 °C
Specific Heat Capacity 0.0920 BTU/lb-°F
Thermal Conductivity 224 BTU-in/hr-ft²-°F
Melting Point <= 1980 °F
Liquidus 1980 °F
Annealing Point 900 - 1400 °F
 
Processing PropertiesOriginal ValueComments
Hot-Working Temperature 1400 - 1600 °F
 
Component Elements PropertiesOriginal ValueComments
Copper, Cu >= 99.9 %
Silver, Ag >= 0.085 %
 
Descriptive Properties
Cold Work (%)162 in
 351 in
 400.25 in
US EPA Registered AntimicrobialYes

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

MC11600x1 / 292694

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.