MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Pearl Engineering PEPLPET B-101C PET Sheet Grade
Categories: Polymer; Thermoplastic; Polyester, TP; Polyethylene Terephthalate (PET)

Material Notes: A sheet grade polymer used in thick films.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.39 - 1.41 g/ccPEPL-10-W-21
Bulk Density 0.800 - 0.900 g/ccPEPL-10-W-67
Bead Size 2.20 mmchip size, length; PEPL-10-W-71
 2.60 mmchip size, D2; PEPL-10-W-71
 3.10 mmchip size, D1; PEPL-10-W-71
Viscosity Test 70 - 74 cm³/gIntrinsic; PEPL-10-W-15
Molecular Weight 43000 g/molWeight average M
 215000 g/molNumber average M
Ash 0.025 %PEPL-10-W-66
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 1.00e+18 ohm-cm
Dielectric Constant 3.3
 
Thermal PropertiesOriginal ValueComments
Heat of Fusion <= 65.0 J/gDensity at 1.38 g/cc
Specific Heat Capacity 1.10 J/g-°C
@Temperature 20.0 °C
 1.37 J/g-°C
@Temperature 80.0 °C
 1.44 J/g-°C
@Temperature 100 °C
 1.82 J/g-°C
@Temperature 200 °C
 2.05 J/g-°C
@Temperature 280 °C
Thermal Conductivity 0.213 W/m-K
@Temperature 280 °C
liquid
 0.242 W/m-K
@Temperature 20.0 °C
solid
Melting Point 248 - 250 °CPEPL-10-W-19
Maximum Service Temperature, Air <= 70.0 °C
Glass Transition Temp, Tg 79.0 °CPEPL-10-W-19
Flash Point 480 °C
 
Processing PropertiesOriginal ValueComments
Moisture Content <= 0.20 %when packed; PEPL-10-W-13
 
Descriptive Properties
Acetaldehydes (ppm)<1PEPL-10-W-20
Chips per Gram58-66PEPL-10-W-13
COOH end groups (mval/kg)<30PEPL-10-W-16
Fines (ppm)<100PEPL-10-W-65

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Geon® Performance Solutions 87725 Sheet PVC
Kostat ICP-STAT ICD-1001 PET Sheet
OCTAL DPET™ PET Sheet
Overview of materials for PVC, Sheet Grade
Armacell Ensolite™ IFC-400 Continuous Rolls/Sheets, PVC/NBR

PPEPL007 / 79830

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.