MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

ArcelorMittal Torque 27-16 Electrical Steel
Categories: Metal; Ferrous Metal; Alloy Steel

Material Notes: Properties: The iCARe™ Torque product family comes with guaranteed losses at 400Hz and indicative maximum values at 700Hz. These values are representative of the steel’s behaviour at high frequencies.

Advantages: Torque grades assist flux generation, allowing the motor to develop more mechanical output. If mechanical output is not an issue, permanent magnet or copper winding can be reduced to save on costs

Applications: Torque grades are suitable for machines which need high torque at low speeds. They provide the fast acceleration required by hybrid and electric vehicles.

Recommendations for use: Torque grades can be used immediately after lamination punching. The effect of punching can be eliminated if a stress relief annealing is applied. This optimises the performance of the Torque grades in applications with fine teeth. It can also provide substantial performance improvements in the lower frequency range. To achieve these effects, a C5 type coating is advised. Torque stacks can be produced using existing assembly techniques such as interlocking or welding.

Information provided by ArcelorMittal

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.65 g/cc0.276 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Vickers 170 - 200170 - 200L direction
 170 - 200170 - 200T direction
Tensile Strength, Ultimate 470 - 510 MPa68200 - 74000 psiL direction
 490 - 530 MPa71100 - 76900 psiT direction
Tensile Strength, Yield 340 - 380 MPa49300 - 55100 psiL direction
 360 - 400 MPa52200 - 58000 psiT direction
Elongation at Break 13 - 28 %13 - 28 %L direction
 13 - 28 %13 - 28 %T direction
 
Magnetic PropertiesMetricEnglishComments
Core Loss  <= 16.0 W/kg
@Frequency 400 Hz
<= 7.26 W/lb
@Frequency 400 Hz
at 1T, Guaranteed
 <= 38.0 W/kg
@Frequency 700 Hz
<= 17.2 W/lb
@Frequency 700 Hz
at 1T, Indicative
 
Descriptive Properties
Anisotropy>15%400 Hz at 1T
Polarization>1.55 Tat 2,500 A/m
 >1.65 Tat 5,000 A/m
 >1.76 Tat 10,000 A/m

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
AK Steel CARLITE® M-5 Grain Oriented Electrical Steel
AK Steel DI-MAX® M-36 Nonoriented Electrical Steel
AK Steel CARLITE® M-5 Grain Oriented Electrical Steel (Extended Electro-Magnetic Data)
AK Steel DI-MAX® M-15 Nonoriented Electrical Steel
AK Steel DI-MAX® M-19 Nonoriented Electrical Steel

NARCE119 / 160027

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.