MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Epoxies, Etc 20-3302NCLV Water Clear Optically Transparent Epoxy Potting Compound & Adhesive
Categories: Polymer; Thermoset; Epoxy

Material Notes: Description: 20-3302 is a two component, ultra clear epoxy system. It provides excellent optical transmission along with outstanding adhesion and electrical properties. This high purity grade polymer system is formulated with proprietary ultraviolet protectors to minimize yellowing of the cured epoxy. This adhesive\potting compound, when UV aged in a QUV Weatherometer, outperforms other commercially available epoxy systems. 20-3302 is a low viscosity system designed for L.E.D. encapsulating, fiber optics, and any potting or adhesive application requiring optimum clarity. This epoxy system also provides a bubble free and glass smooth finish. 20-3302NCLV is a lower viscosity version of 20-3302. Both resins utilize the same curing agent.

Features:

  • Low viscosity
  • Water clear
  • Outstanding electrical properties
  • Bubble free castings

Information provided by Epoxies, Etc

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 0.960 g/cc0.960 g/ccCatalyst
 1.10 g/cc1.10 g/ccResin
Viscosity 250 cP250 cPMixed
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 8585
Shear Strength 15.5 MPa2250 psiLap
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity >= 3.50e+14 ohm-cm>= 3.50e+14 ohm-cm
Dielectric Constant 3.13.1
Dielectric Strength 19.7 kV/mm500 kV/in
 
Thermal PropertiesMetricEnglishComments
CTE, linear 62.0 µm/m-°C
@Temperature 30.0 - 90.0 °C
34.4 µin/in-°F
@Temperature 86.0 - 194 °F
Maximum Service Temperature, Air 135 °C275 °F
Minimum Service Temperature, Air -45.0 °C-49.0 °F
 
Optical PropertiesMetricEnglishComments
Refractive Index 1.5641.564
Transmission, Visible 90 %90 %3000 angstroms
 98 - 99 %98 - 99 %3100 angstroms to 2.5 microns
 
Processing PropertiesMetricEnglishComments
Cure Time  60.0 - 120 min
@Temperature 125 °C
1.00 - 2.00 hour
@Temperature 257 °F
 1440 min
@Temperature 25.0 °C
24.0 hour
@Temperature 77.0 °F
Pot Life 30.0 - 45.0 min
@Load 0.100 kg
30.0 - 45.0 min
@Load 0.221 lb
 
Descriptive Properties
ColorWater clear
Mix Ratio100:50by weight (Resin:Hardener)
 100:60by volume (Resin:Hardener)

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PFEPOX039 / 316716

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.