Physical Properties | Metric | English | Comments |
---|
Specific Gravity | 1.24 g/cc | 1.24 g/cc |
Linear Mold Shrinkage, Flow | 0.0080 cm/cm @Thickness 2.54 mm | 0.0080 in/in @Thickness 0.100 in |
Linear Mold Shrinkage, Transverse | 0.0080 cm/cm @Thickness 2.54 mm | 0.0080 in/in @Thickness 0.100 in |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Shore D | 70 | 70 |
| 65 @Temperature 168 °C | 65 @Temperature 334 °F |
| 65 @Temperature 504 °C | 65 @Temperature 939 °F |
| 66 @Temperature 336 °C | 66 @Temperature 637 °F |
| 69 @Temperature 70.0 °C | 69 @Temperature 158 °F |
| 69 @Temperature 168 °C | 69 @Temperature 334 °F |
| 69 @Temperature 336 °C | 69 @Temperature 637 °F |
| 70 @Temperature 70.0 °C | 70 @Temperature 158 °F |
| 72 @Temperature 504 °C | 72 @Temperature 939 °F |
| 64 @Treatment Temp. 168 °C, Time 100 sec | 64 @Treatment Temp. 334 °F, Time 0.0278 hour |
| 65 @Treatment Temp. 168 °C, Time 100 sec | 65 @Treatment Temp. 334 °F, Time 0.0278 hour |
| 65 @Treatment Temp. 336 °C, Time 100 sec | 65 @Treatment Temp. 637 °F, Time 0.0278 hour |
| 65 @Treatment Temp. 504 °C, Time 100 sec | 65 @Treatment Temp. 939 °F, Time 0.0278 hour |
| 66 @Treatment Temp. 70.0 °C, Time 100 sec | 66 @Treatment Temp. 158 °F, Time 0.0278 hour |
| 66 @Treatment Temp. 336 °C, Time 100 sec | 66 @Treatment Temp. 637 °F, Time 0.0278 hour |
| 67 @Treatment Temp. 168 °C, Time 100 sec | 67 @Treatment Temp. 334 °F, Time 0.0278 hour |
| 68 @Treatment Temp. 336 °C, Time 100 sec | 68 @Treatment Temp. 637 °F, Time 0.0278 hour |
| 68 @Treatment Temp. 504 °C, Time 100 sec | 68 @Treatment Temp. 939 °F, Time 0.0278 hour |
| 69 @Treatment Temp. 70.0 °C, Time 100 sec | 69 @Treatment Temp. 158 °F, Time 0.0278 hour |
| 69 @Treatment Temp. 504 °C, Time 100 sec | 69 @Treatment Temp. 939 °F, Time 0.0278 hour |
| 71 @Treatment Temp. 70.0 °C, Time 100 sec | 71 @Treatment Temp. 158 °F, Time 0.0278 hour |
Tensile Strength at Break | 56.6 MPa | 8210 psi |
| 53.77 MPa @Time 605000 sec | 7799 psi @Time 168 hour |
| 54.336 MPa @Time 252000 sec | 7880.8 psi @Time 70.0 hour |
| 55.468 MPa @Time 1.81e+6 sec | 8045.0 psi @Time 504 hour |
| 56.6 MPa @Time 1.21e+6 sec | 8210 psi @Time 336 hour |
| 58.298 MPa @Time 605000 sec | 8455.4 psi @Time 168 hour |
| 61.128 MPa @Time 1.21e+6 sec | 8865.9 psi @Time 336 hour |
| 61.694 MPa @Time 1.81e+6 sec | 8948.0 psi @Time 504 hour |
| 62.26 MPa @Time 252000 sec | 9030 psi @Time 70.0 hour |
| 57.912 MPa @Treatment Temp. 100 °C, Time 1.21e+6 sec | 8399.4 psi @Treatment Temp. 212 °F, Time 336 hour |
| 60.058 MPa @Treatment Temp. 100 °C, Time 252000 sec | 8710.7 psi @Treatment Temp. 212 °F, Time 70.0 hour |
| 60.562 MPa @Treatment Temp. 100 °C, Time 605000 sec | 8783.8 psi @Treatment Temp. 212 °F, Time 168 hour |
| 61.128 MPa @Treatment Temp. 100 °C, Time 1.81e+6 sec | 8865.9 psi @Treatment Temp. 212 °F, Time 504 hour |
| 61.694 MPa @Treatment Temp. 100 °C, Time 1.21e+6 sec | 8948.0 psi @Treatment Temp. 212 °F, Time 336 hour |
| 62.26 MPa @Treatment Temp. 100 °C, Time 605000 sec | 9030 psi @Treatment Temp. 212 °F, Time 168 hour |
| 66.222 MPa @Treatment Temp. 100 °C, Time 252000 sec | 9604.7 psi @Treatment Temp. 212 °F, Time 70.0 hour |
| 67.92 MPa @Treatment Temp. 100 °C, Time 1.81e+6 sec | 9851 psi @Treatment Temp. 212 °F, Time 504 hour |
| 67.92 MPa @Treatment Temp. 100 °C, Time 252000 sec | 9851 psi @Treatment Temp. 212 °F, Time 70.0 hour |
| 68.486 MPa @Treatment Temp. 100 °C, Time 1.81e+6 sec | 9933.1 psi @Treatment Temp. 212 °F, Time 504 hour |
| 73.014 MPa @Treatment Temp. 100 °C, Time 605000 sec | 10590 psi @Treatment Temp. 212 °F, Time 168 hour |
| 74.712 MPa @Treatment Temp. 100 °C, Time 1.21e+6 sec | 10836 psi @Treatment Temp. 212 °F, Time 336 hour |
Tensile Stress at Strain | 28.3 MPa @Strain 50 % | 4100 psi @Strain 50 % |
| 29.0 MPa @Strain 100 % | 4210 psi @Strain 100 % |
| 42.8 MPa @Strain 300 % | 6210 psi @Strain 300 % |
| 26.68 MPa @Strain 100 %, Temperature 100 °C | 3870 psi @Strain 100 %, Temperature 212 °F |
| 27.26 MPa @Strain 100 %, Temperature 100 °C | 3954 psi @Strain 100 %, Temperature 212 °F |
| 28.13 MPa @Strain 100 %, Temperature 100 °C | 4080 psi @Strain 100 %, Temperature 212 °F |
| 28.42 MPa @Strain 100 %, Temperature 100 °C | 4122 psi @Strain 100 %, Temperature 212 °F |
| 28.71 MPa @Strain 100 %, Temperature 100 °C | 4164 psi @Strain 100 %, Temperature 212 °F |
| 28.71 MPa @Strain 100 %, Temperature 100 °C | 4164 psi @Strain 100 %, Temperature 212 °F |
| 29.0 MPa @Strain 100 %, Temperature 100 °C | 4210 psi @Strain 100 %, Temperature 212 °F |
| 29.29 MPa @Strain 100 %, Temperature 100 °C | 4248 psi @Strain 100 %, Temperature 212 °F |
| 29.58 MPa @Strain 100 %, Temperature 100 °C | 4290 psi @Strain 100 %, Temperature 212 °F |
| 29.58 MPa @Strain 100 %, Temperature 100 °C | 4290 psi @Strain 100 %, Temperature 212 °F |
| 29.58 MPa @Strain 100 %, Temperature 100 °C | 4290 psi @Strain 100 %, Temperature 212 °F |
| 31.9 MPa @Strain 100 %, Temperature 100 °C | 4630 psi @Strain 100 %, Temperature 212 °F |
| 38.192 MPa @Strain 300 %, Temperature 100 °C | 5539.3 psi @Strain 300 %, Temperature 212 °F |
| 38.192 MPa @Strain 300 %, Temperature 100 °C | 5539.3 psi @Strain 300 %, Temperature 212 °F |
| 41.944 MPa @Strain 300 %, Temperature 100 °C | 6083.5 psi @Strain 300 %, Temperature 212 °F |
| 43.656 MPa @Strain 300 %, Temperature 100 °C | 6331.8 psi @Strain 300 %, Temperature 212 °F |
| 44.512 MPa @Strain 300 %, Temperature 100 °C | 6455.9 psi @Strain 300 %, Temperature 212 °F |
| 44.512 MPa @Strain 300 %, Temperature 100 °C | 6455.9 psi @Strain 300 %, Temperature 212 °F |
| 45.468 MPa @Strain 300 %, Temperature 100 °C | 6594.6 psi @Strain 300 %, Temperature 212 °F |
| 46.224 MPa @Strain 300 %, Temperature 100 °C | 6704.2 psi @Strain 300 %, Temperature 212 °F |
| 47.936 MPa @Strain 300 %, Temperature 100 °C | 6952.5 psi @Strain 300 %, Temperature 212 °F |
| 48.056 MPa @Strain 300 %, Temperature 100 °C | 6969.9 psi @Strain 300 %, Temperature 212 °F |
| 51.196 MPa @Strain 300 %, Temperature 100 °C | 7425.4 psi @Strain 300 %, Temperature 212 °F |
| 51.624 MPa @Strain 300 %, Temperature 100 °C | 7487.4 psi @Strain 300 %, Temperature 212 °F |
| 22.91 MPa @Strain 100 %, Time 1.81e+6 sec | 3323 psi @Strain 100 %, Time 504 hour |
| 23.78 MPa @Strain 100 %, Time 1.21e+6 sec | 3449 psi @Strain 100 %, Time 336 hour |
| 27.26 MPa @Strain 100 %, Time 605000 sec | 3954 psi @Strain 100 %, Time 168 hour |
| 27.84 MPa @Time 252000 sec, Strain 100 % | 4038 psi @Time 70.0 hour, Strain 100 % |
| 27.84 MPa @Time 252000 sec, Strain 100 % | 4038 psi @Time 70.0 hour, Strain 100 % |
| 28.13 MPa @Strain 100 %, Time 605000 sec | 4080 psi @Strain 100 %, Time 168 hour |
| 28.13 MPa @Strain 100 %, Time 1.21e+6 sec | 4080 psi @Strain 100 %, Time 336 hour |
| 28.71 MPa @Strain 100 %, Time 1.81e+6 sec | 4164 psi @Strain 100 %, Time 504 hour |
| 41.088 MPa @Time 605000 sec, Strain 300 % | 5959.3 psi @Time 168 hour, Strain 300 % |
| 41.088 MPa @Strain 300 %, Time 1.21e+6 sec | 5959.3 psi @Strain 300 %, Time 336 hour |
| 41.944 MPa @Time 252000 sec, Strain 300 % | 6083.5 psi @Time 70.0 hour, Strain 300 % |
| 41.944 MPa @Strain 300 %, Time 1.81e+6 sec | 6083.5 psi @Strain 300 %, Time 504 hour |
| 42.372 MPa @Time 252000 sec, Strain 300 % | 6145.6 psi @Time 70.0 hour, Strain 300 % |
| 42.372 MPa @Strain 300 %, Time 1.81e+6 sec | 6145.6 psi @Strain 300 %, Time 504 hour |
| 43.712 MPa @Strain 300 %, Time 1.21e+6 sec | 6339.9 psi @Strain 300 %, Time 336 hour |
| 52.48 MPa @Time 605000 sec, Strain 300 % | 7612 psi @Time 168 hour, Strain 300 % |
Elongation at Break | 400 % | 400 % |
| 372 % @Time 1.21e+6 sec | 372 % @Time 336 hour |
| 396 % @Time 1.81e+6 sec | 396 % @Time 504 hour |
| 400 % @Time 252000 sec | 400 % @Time 70.0 hour |
| 400 % @Time 605000 sec | 400 % @Time 168 hour |
| 440 % @Time 1.81e+6 sec | 440 % @Time 504 hour |
| 443 % @Time 605000 sec | 443 % @Time 168 hour |
| 448 % @Time 1.21e+6 sec | 448 % @Time 336 hour |
| 460 % @Time 252000 sec | 460 % @Time 70.0 hour |
| 384 % @Treatment Temp. 100 °C, Time 605000 sec | 384 % @Treatment Temp. 212 °F, Time 168 hour |
| 412 % @Treatment Temp. 100 °C, Time 252000 sec | 412 % @Treatment Temp. 212 °F, Time 70.0 hour |
| 412 % @Treatment Temp. 100 °C, Time 605000 sec | 412 % @Treatment Temp. 212 °F, Time 168 hour |
| 412 % @Treatment Temp. 100 °C, Time 1.21e+6 sec | 412 % @Treatment Temp. 212 °F, Time 336 hour |
| 412 % @Treatment Temp. 100 °C, Time 1.81e+6 sec | 412 % @Treatment Temp. 212 °F, Time 504 hour |
| 416 % @Treatment Temp. 100 °C, Time 1.21e+6 sec | 416 % @Treatment Temp. 212 °F, Time 336 hour |
| 432 % @Treatment Temp. 100 °C, Time 252000 sec | 432 % @Treatment Temp. 212 °F, Time 70.0 hour |
| 468 % @Treatment Temp. 100 °C, Time 1.81e+6 sec | 468 % @Treatment Temp. 212 °F, Time 504 hour |
| 468 % @Treatment Temp. 100 °C, Time 252000 sec | 468 % @Treatment Temp. 212 °F, Time 70.0 hour |
| 476 % @Treatment Temp. 100 °C, Time 605000 sec | 476 % @Treatment Temp. 212 °F, Time 168 hour |
| 544 % @Treatment Temp. 100 °C, Time 1.21e+6 sec | 544 % @Treatment Temp. 212 °F, Time 336 hour |
| 604 % @Treatment Temp. 100 °C, Time 1.81e+6 sec | 604 % @Treatment Temp. 212 °F, Time 504 hour |
Elongation at Yield | 1.132 % | 1.132 % |
| 1.132 % | 1.132 % |
| 1.698 % | 1.698 % |
| 2.264 % | 2.264 % |
| 2.83 % | 2.83 % |
| 3.458 % | 3.458 % |
| 3.962 % | 3.962 % |
| 4.528 % | 4.528 % |
| 4.528 % | 4.528 % |
| 5.094 % | 5.094 % |
| 5.094 % | 5.094 % |
| 5.66 % | 5.66 % |
| 5.66 % | 5.66 % |
| 9.622 % | 9.622 % |
| 11.32 % | 11.32 % |
| 11.32 % | 11.32 % |
| 11.886 % | 11.886 % |
| 16.414 % | 16.414 % |
| 18.112 % | 18.112 % |
Flexural Modulus | 0.103 GPa @Temperature 70.0 °C | 14.9 ksi @Temperature 158 °F |
| 0.724 GPa @Temperature 23.0 °C | 105 ksi @Temperature 73.4 °F |
| 2.91 GPa @Temperature -30.0 °C | 422 ksi @Temperature -22.0 °F |
Compressive Strength | 3.80 MPa | 551 psi |
| 13.1 MPa | 1900 psi |
| 21.7 MPa | 3150 psi |
| 25.9 MPa | 3760 psi |
| 29.3 MPa | 4250 psi |
| 33.8 MPa | 4900 psi |
| 65.8 MPa | 9540 psi |
Resilience | 55 | 55 |
Tear Strength | 228 kN/m | 1300 pli |
Taber Abrasion, mg/1000 Cycles | 90 @Load 1.00 kg | 90 @Load 2.20 lb |
Compression Set | 30 % @Temperature 23.0 °C, Time 79200 sec | 30 % @Temperature 73.4 °F, Time 22.0 hour |
| 45 % @Temperature 70.0 °C, Time 79200 sec | 45 % @Temperature 158 °F, Time 22.0 hour |
| 50 % @Temperature 23.0 °C, Time 79200 sec | 50 % @Temperature 73.4 °F, Time 22.0 hour |
| 85 % @Temperature 70.0 °C, Time 79200 sec | 85 % @Temperature 158 °F, Time 22.0 hour |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear | 99.0 µm/m-°C | 55.0 µin/in-°F |
Deflection Temperature at 0.46 MPa (66 psi) | 46.0 °C | 115 °F |
Deflection Temperature at 1.8 MPa (264 psi) | 38.0 °C | 100 °F |
Vicat Softening Point | 158 °C | 316 °F |
Brittleness Temperature | >= -55.6 °C | >= -68.0 °F |
Glass Transition Temp, Tg | 0.000 °C | 32.0 °F |
|
Processing Properties | Metric | English | Comments |
---|
Rear Barrel Temperature | 210 - 235 °C | 410 - 455 °F |
Middle Barrel Temperature | 210 - 240 °C | 410 - 464 °F |
Front Barrel Temperature | 215 - 240 °C | 419 - 464 °F |
Nozzle Temperature | 215 - 240 °C | 419 - 464 °F |
Melt Temperature | 220 - 240 °C | 428 - 464 °F |
Mold Temperature | 15.0 - 40.0 °C | 59.0 - 104 °F |
Injection Pressure | 41.4 - 103 MPa | 6000 - 15000 psi |
Back Pressure | <= 1.38 MPa | <= 200 psi |
Cushion | <= 0.317 cm | <= 0.125 in |
|
Compliance Properties | Metric | English | Comments |
---|
FDA | Yes | Yes |