MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Omnia Plastica PPS GF40 Polyphenylenesulphide
Categories: Polymer; Thermoplastic; Polyphenylene Sulfide (PPS); Polyphenylene Sulfide (PPS) with 40% Glass Fiber Filler

Material Notes: Crystalline polymer based on polyphenylene sulfide with the addition of 40% glass-fibre. Very high rigidity, stiffness and flexural strength. The temperature resistance is very high: up to 240° C. Its abrasion resistance is among the very best. It is used for small precision parts where a very high dimensional stability is required in both the electrical and nuclear industries.

Features:

  • High temperature resistance (beyond 240° C.)
  • Modulus of elasticity and flexural strength are very high
  • Excellent abrasion resistance
  • Flame resistant
  • Electrical properties
  • Colour: brown
Weak Point:
  • Very high rigidity and brittleness
  • Difficult to machine
Application:
  • Mechanical: the dimensional stability and heat resistance are both excellent and the flexural and compressive strength are exceptional. Components have very good wear resistance but are highly brittle. It is used for high performance small parts such as bearings, precision gears, etc, at both low and high temperatures.
  • Electrical: very good insulating power and dielectric properties make it irreplaceable for many applications in this field.
  • Chemical: very good chemical resistance.
  • Food contact: it is not used in contact with food

Information provided by Omnia Plastica s.p.a. for semifinished products such as sheet, rod, and tube.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.64 g/ccISO.1183 DIN.53479
Moisture Absorption at Equilibrium 0.00 %50% relative humidity
Water Absorption at Saturation 0.10 %23°C
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell R 123dry sample; ISO2039.2
Ball Indentation Hardness 400 MPaISO2039.1 DIN.53456
Tensile Strength at Break 165 MPaISO.527 DIN.53455
Elongation at Break 1.0 %ISO.527 DIN.53455
Tensile Modulus 14.0 GPaISO.527 DIN.53455
Compressive Strength 35.0 MPa1% strain over 1000 hours; ISO.899 DIN.53444
Charpy Impact Unnotched 4.00 J/cm²7.5 J; ISO.R179 DIN.53453
Charpy Impact, Notched 0.800 J/cm²ISO179/3C DIN.53453
Coefficient of Friction, Dynamic 0.50on dry ground steel; load =0.05MPa; speed =0.6 m/s
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+15 ohm-cmISO.93 DIN.53482
Dielectric Constant 4.0
@Frequency 1e+6 Hz
ISO.250 DIN.53483
Dielectric Strength 20.0 kV/mmISO.243 DIN.53481
Dissipation Factor 0.0040
@Frequency 1e+6 Hz
ISO.250 DIN.53483
 
Thermal PropertiesOriginal ValueComments
CTE, linear 20.0 µm/m-°C
@Temperature 23.0 - 60.0 °C
Thermal Conductivity 0.200 W/m-KDIN.52612
Melting Point 285 °C
Maximum Service Temperature, Air 230 °CContinuous; 5000 hours based on a tensile stress of 50% at 23° C.
 260 °Cshort period, no load
Deflection Temperature at 1.8 MPa (264 psi) 260 °CISO.75 DIN.53461
Minimum Service Temperature, Air -50.0 °Cimpact conditions and heavy loads not considered
Flammability, UL94 V-0

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Celanese Celstran® PPS-GF40-01 PPS, 40% Glass Reinforced
Celanese Celstran® PPS-GF40-01 AD3002 Black PPS, 40% Glass Reinforced
LG Chemical LUSEP GP2400 PPS+GF40%, General Purpose
Techmer ES HiFill® PPS GF40 BK 40% Glass Filled
Techmer ES HiFill® PPS GF40 TL13 40% Glass Filled

POMNIA43 / 55632

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.