MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Multibase Multi-Pro® 2518 CU 25% Mineral Filled Polypropylene
Categories: Polymer; Thermoplastic; Polypropylene (PP); Polypropylene, Mineral Reinforced

Material Notes: Multi-Pro 2518 CU is a mineral reinforced polypropylene compound offering overall balanced impact and stiffness properties. This material is specially formulated with UV stabilization for outdoor exposure and is particularly suited for lawn furniture applications.

Data provided by Multibase.

Key Words: PP
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.08 g/ccASTM D792-91
Linear Mold Shrinkage 0.0090 cm/cmASTM D955-89
Melt Flow 18 g/10 min(Condition L) ASTM D-1238-94a
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 7210 sec; ASTM D-2240-95
Tensile Strength, Ultimate 24.1 MPaASTM D638-95
Elongation at Break 150 %ASTM D638-95
Flexural Modulus 1.724 GPaMethod 1, Proc. B; ASTM D-790-95
Izod Impact, Notched 0.530 J/cmASTM D256-93a
Gardner Impact 5.60 JASTM D5420-93
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 0.46 MPa (66 psi) 102 °CASTM D648-95
Deflection Temperature at 1.8 MPa (264 psi) 63.0 °CASTM D648-95
 
Optical PropertiesOriginal ValueComments
Gloss 72 %ASTM D2457-90

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Addiplast Addilene H 220 M40 Polypropylene Homopolymer
ExxonMobil PP1043F Mineral-filled Homopolymer
A. Schulman CPP30GF33BK 30% Mineral Filled, Heat-Stabilized, Homopolymer Polypropylene
Pasargad Polymer Peyvand Pasalen 3P-H3240B Polypropylene, 40% Mineral Filled Reinforced
LG Chemical LUPOL GP3400 PP+MF40%

PLA257 / 49654

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.