MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Teknor Apex Sarlink® TPV 24564 Thermoplastic Vulcanizate
Categories: Polymer; Thermoplastic; Elastomer, TPE; Thermoplastic Vulcanizate Elastomer (TPV)

Material Notes: Notes: Sarlink TPV 24564 is a high performance thermoplastic vulcanizate used in a variety of automotive, consumer and industrial applications. This product is a medium hardness, low density, UV stabilized grade designed for injection molding.

Availability: Africa & Middle East; Asia Pacific; Europe; Latin America; North America

Features: Chemical Resistant; Good Adhesion; Good Flexibility; Good Moldability; Good Toughness; Low Density; Low Specific Gravity; Medium Hardness; Resilient; UV Stabilized; Weather Resistant

Uses: Appliance Components; Automotive Applications; Expansion Joint; Gaskets; Glazing; Grommets; Industrial Applications; O-rings; Plugs; Rubber Replacement; Shock Absorbing Pads; Weatherstripping

Agency Ratings: UL 94

RoHS Compliance: RoHS Compliant

UL File Number: QMFZ2.E54709

Form: Pellets

Processing Method: Injection Molding

Information provided by Teknor Apex

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.940 g/cc0.0340 lb/in³ISO 1183
Melt Flow 4.5 g/10 min
@Load 2.16 kg,
Temperature 230 °C
4.5 g/10 min
@Load 4.76 lb,
Temperature 446 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 6868ASTM D2240
 64
@Time 5.00 sec
64
@Time 0.00139 hour
ASTM D2240
Tensile Strength at Break 5.17 MPa750 psiISO 37
 4.34 MPa
@Time 7.20e+6 sec
630 psi
@Time 2000 hour
Xenon Weatherometer; SAE J1960
Elongation at Break 350 %350 %ISO 37
 273 %
@Time 7.20e+6 sec
273 %
@Time 2000 hour
Xenon Weatherometer; SAE J1960
Compression Set  23 %
@Temperature 22.8 °C,
Time 79200 sec
23 %
@Temperature 73.0 °F,
Time 22.0 hour
ASTM D395
 36 %
@Temperature 70.0 °C,
Time 79200 sec
36 %
@Temperature 158 °F,
Time 22.0 hour
ASTM D395
 
Thermal PropertiesMetricEnglishComments
UL RTI, Electrical 50.0 °C122 °FUL 746
UL RTI, Mechanical with Impact 50.0 °C122 °FUL 746
UL RTI, Mechanical without Impact 50.0 °C122 °FUL 746
Flammability, UL94 HB
@Thickness 1.52 mm
HB
@Thickness 0.0600 in
All Colors
 
Processing PropertiesMetricEnglishComments
Processing Temperature 190 - 230 °C374 - 446 °FInjection, Melt
Rear Barrel Temperature 173 - 213 °C344 - 416 °FInjection
Middle Barrel Temperature 179 - 219 °C354 - 426 °FInjection
Front Barrel Temperature 184 - 224 °C364 - 436 °FInjection
Nozzle Temperature 190 - 230 °C374 - 446 °FInjection
Mold Temperature 35.0 - 60.0 °C95.0 - 140 °FInjection
Injection Pressure 1.38 - 6.89 MPa200 - 1000 psiInjection
Back Pressure 0.172 - 0.862 MPa25.0 - 125 psiInjection
Cushion 0.381 - 2.54 cm0.150 - 1.00 inInjection
Screw Speed 50 - 120 rpm50 - 120 rpmInjection
 
Descriptive Properties
AppearanceNatural Color
 Opaque

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PTEKNQ1192 / 237683

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.