MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Iran Petrochemical (PCC) GPPS 1540 Polystyrene
Categories: Polymer; Thermoplastic; Polystyrene (PS); Polystyrene, Extrusion Grade; Polystyrene, Molded, Unreinforced

Material Notes: GPPS 1540 is an easy flowing crystal polystyrene designed for extrusion or injection applications. In extrusion, it improves extruder output and thermoforming cycle times when mixed with a high impact polystyrene. It is particularly suitable for glossy-layer co-extrusion.

Applications: impact dilution, gloss layer in co-extrusion, packaging articles, medical applications, office equipment

Information provided by Iran Petrochemical Commercial Co.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.04 g/cc0.0376 lb/in³
Moisture Absorption <= 0.100 %<= 0.100 %ASTM D570
Linear Mold Shrinkage 0.0040 - 0.0070 cm/cm0.0040 - 0.0070 in/inASTM D570
Melt Flow 11 g/10 min
@Load 5.00 kg,
Temperature 200 °C
11 g/10 min
@Load 11.0 lb,
Temperature 392 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 45.0 MPa6530 psiASTM D638
Elongation at Break 2.0 %2.0 %ASTM D638
Tensile Modulus 3.10 GPa450 ksiASTM D638
Flexural Modulus 3.00 GPa435 ksiASTM D790
 
Thermal PropertiesMetricEnglishComments
Vicat Softening Point >= 89.5 °C>= 193 °FASTM D1525
 
Optical PropertiesMetricEnglishComments
Refractive Index 1.5911.591ISO

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
INEOS Styrolution PS 147F GPPS
Iran Petrochemical (PCC) GPPS 1160 Polystyrene
Supreme Petrochem SC 203EL General Purpose Polystyrene
INEOS Styrolution PS 116 N/L GPPS
Iran Petrochemical (PCC) Arak BL4 HDPE

PIPC343 / 149777

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.