MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Overview of materials for Acrylonitrile Butadiene Styrene (ABS), Molded
Categories: Polymer; Thermoplastic; ABS Polymer; Acrylonitrile Butadiene Styrene (ABS), Molded

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "Acrylonitrile Butadiene Styrene (ABS), Molded". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 0.882 - 3.50 g/ccAverage value: 1.07 g/cc Grade Count:774
Water Absorption 0.0250 - 2.30 %Average value: 0.383 % Grade Count:85
Moisture Absorption at Equilibrium 0.100 - 0.300 %Average value: 0.232 % Grade Count:26
Water Absorption at Saturation 0.00950 - 1.03 %Average value: 0.561 % Grade Count:14
Maximum Moisture Content 0.0100 - 0.150Average value: 0.0459 Grade Count:71
Linear Mold Shrinkage 0.000 - 0.0290 cm/cmAverage value: 0.00533 cm/cm Grade Count:581
Linear Mold Shrinkage, Transverse 0.00200 - 0.00900 cm/cmAverage value: 0.00522 cm/cm Grade Count:52
Melt Flow 0.0800 - 125 g/10 minAverage value: 16.5 g/10 min Grade Count:805
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell M 53.0 - 92.0Average value: 71.8 Grade Count:4
Hardness, Rockwell R 13.0 - 122Average value: 108 Grade Count:431
Hardness, Shore D 79.0 - 103Average value: 87.0 Grade Count:3
Ball Indentation Hardness 70.0 - 120 MPaAverage value: 101 MPa Grade Count:68
Tensile Strength, Ultimate 2.60 - 73.1 MPaAverage value: 41.0 MPa Grade Count:346
 20.0 - 43.0 MPa
@Temperature 60.0 - 90.0 °C
Average value: 31.8 MPa Grade Count:2
Tensile Strength, Yield 2.00 - 77.0 MPaAverage value: 44.8 MPa Grade Count:624
Elongation at Break 1.40 - 110 %Average value: 28.5 % Grade Count:493
Elongation at Yield 1.70 - 40.0 %Average value: 3.66 % Grade Count:189
Modulus of Elasticity 0.778 - 21.2 GPaAverage value: 2.35 GPa Grade Count:356
Flexural Yield Strength 0.379 - 655 MPaAverage value: 70.6 MPa Grade Count:626
Flexural Modulus 0.0241 - 6.89 GPaAverage value: 2.33 GPa Grade Count:699
 1.50 - 4.00 GPa
@Temperature 60.0 - 90.0 °C
Average value: 2.84 GPa Grade Count:2
Poissons Ratio 0.360 - 0.380Average value: 0.364 Grade Count:5
Izod Impact, Notched 0.100 - 7.85 J/cmAverage value: 2.41 J/cm Grade Count:516
 0.350 - 3.00 J/cm
@Temperature -50.0 - 0.000 °C
Average value: 1.00 J/cm Grade Count:23
 0.290 - 2.35 J/cm
@Temperature -40.0 - 0.000 °C
Average value: 1.00 J/cm Grade Count:30
 0.290 - 2.35 J/cm
@Thickness 3.17 - 12.7 mm
Average value: 1.00 J/cm Grade Count:30
Izod Impact, Unnotched 1.50 J/cm - NBAverage value: 8.79 J/cm Grade Count:27
 0.600 - 6.47239 J/cm
@Temperature -30.0 - 0.125 °C
Average value: 1.24 J/cm Grade Count:4
 0.392266 - 4.8051 J/cm
@Temperature -30.0 - -20.0 °C
Average value: 1.24 J/cm Grade Count:34
 0.392266 - 4.8051 J/cm
@Thickness 3.20 - 6.40 mm
Average value: 1.24 J/cm Grade Count:34
Izod Impact, Notched (ISO) 1.00 - 45.0 kJ/m²Average value: 18.5 kJ/m² Grade Count:184
 6.00 - 22.0 kJ/m²
@Temperature -40.0 - -20.0 °C
Average value: 9.13 kJ/m² Grade Count:61
 6.00 - 6.00 kJ/m²
@Temperature -40.0 - -40.0 °C
Average value: 9.13 kJ/m² Grade Count:1
 6.00 - 6.00 kJ/m²
@Thickness 4.00 - 4.00 mm
Average value: 9.13 kJ/m² Grade Count:1
Izod Impact, Unnotched (ISO) 39.2 kJ/m² - NBAverage value: 77.2 kJ/m² Grade Count:27
 60.0 - 70.0 kJ/m²
@Temperature -30.0 - -30.0 °C
Average value: 68.0 kJ/m² Grade Count:5
Charpy Impact Unnotched 1.00 J/cm² - NBAverage value: 11.4 J/cm² Grade Count:145
 0.300 J/cm² - NB
@Temperature -40.0 - -20.0 °C
Average value: 7.48 J/cm² Grade Count:96
Charpy Impact, Notched 0.100 - 14.0 J/cm²Average value: 1.90 J/cm² Grade Count:292
 0.200 - 2.40 J/cm²
@Temperature -40.0 - -20.0 °C
Average value: 0.877 J/cm² Grade Count:103
Gardner Impact 1.80 - 22.6 JAverage value: 15.9 J Grade Count:7
Dart Drop, Total Energy 2.37 - 46.3 JAverage value: 28.0 J Grade Count:5
 32.8 - 32.8 J
@Temperature -18.0 - -18.0 °C
Average value: 35.8 J Grade Count:1
 37.3 - 37.3 J
@Temperature -18.0 - -18.0 °C
Average value: 35.8 J Grade Count:1
 37.3 - 37.3 J
@Thickness 3.20 - 3.20 mm
Average value: 35.8 J Grade Count:1
Falling Dart Impact 2.82 - 37.6 JAverage value: 25.3 J Grade Count:9
Instrumented Impact Total Energy 5.40 - 54.0 JAverage value: 39.6 J Grade Count:21
Tensile Creep Modulus, 1 hour 2200 - 2800 MPaAverage value: 2480 MPa Grade Count:4
Tensile Creep Modulus, 1000 hours 1250 - 1900 MPaAverage value: 1640 MPa Grade Count:4
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 1500 - 1.00e+18 ohm-cmAverage value: 1.87e+16 ohm-cm Grade Count:127
Surface Resistance 1000 - 2.00e+17 ohmAverage value: 6.94e+15 ohm Grade Count:120
Static Decay 0.250 - 3.00 secAverage value: 1.24 sec Grade Count:7
Dielectric Constant 2.70 - 3.80Average value: 2.98 Grade Count:54
Dielectric Strength 15.7 - 53.0 kV/mmAverage value: 32.0 kV/mm Grade Count:80
Dissipation Factor 0.00400 - 0.0900Average value: 0.00949 Grade Count:52
Arc Resistance 0.000 - 180 secAverage value: 78.8 sec Grade Count:28
Comparative Tracking Index 92.0 - 600 VAverage value: 561 V Grade Count:93
Hot Wire Ignition, HWI 7.00 - 120 secAverage value: 26.9 sec Grade Count:33
High Amp Arc Ignition, HAI 30.0 - 200 arcsAverage value: 123 arcs Grade Count:33
High Voltage Arc-Tracking Rate, HVTR 0.000 - 150 mm/minAverage value: 34.4 mm/min Grade Count:31
 
Thermal PropertiesOriginal ValueComments
CTE, linear 7.90 - 139 µm/m-°CAverage value: 83.4 µm/m-°C Grade Count:189
CTE, linear, Transverse to Flow 81.0 - 100 µm/m-°CAverage value: 91.4 µm/m-°C Grade Count:15
Specific Heat Capacity 1.60 - 2.13 J/g-°CAverage value: 1.99 J/g-°C Grade Count:7
Thermal Conductivity 0.128 - 0.187 W/m-KAverage value: 0.162 W/m-K Grade Count:19
 0.250 - 0.250 W/m-K
@Temperature 30.0 - 260 °C
Average value: 0.250 W/m-K Grade Count:1
Maximum Service Temperature, Air 50.0 - 109 °CAverage value: 74.9 °C Grade Count:24
Hot Ball Pressure Test 75.0 - 105 °CAverage value: 88.0 °C Grade Count:27
Deflection Temperature at 0.46 MPa (66 psi) 56.0 - 165 °CAverage value: 95.3 °C Grade Count:256
Deflection Temperature at 1.8 MPa (264 psi) 63.9 - 220 °CAverage value: 89.0 °C Grade Count:702
Vicat Softening Point 45.0 - 160 °CAverage value: 99.5 °C Grade Count:571
Heat Distortion Temperature 76.4 - 87.8 °CAverage value: 84.2 °C Grade Count:6
Glass Transition Temp, Tg 105 - 109 °CAverage value: 107 °C Grade Count:9
UL RTI, Electrical 50.0 - 120 °CAverage value: 73.4 °C Grade Count:94
UL RTI, Mechanical with Impact 50.0 - 105 °CAverage value: 71.1 °C Grade Count:85
UL RTI, Mechanical without Impact 50.0 - 120 °CAverage value: 73.2 °C Grade Count:84
Flammability, UL94 HB - 5VAAverage value: 1.50 Grade Count:511
Oxygen Index 19.0 - 30.0 %Average value: 21.6 % Grade Count:5
Glow Wire Test 600 - 960 °CAverage value: 673 °C Grade Count:49
 
Optical PropertiesOriginal ValueComments
Haze 2.00 - 4.00 %Average value: 2.74 % Grade Count:7
Gloss 30.0 - 98.0 %Average value: 84.0 % Grade Count:57
Yellow Index -1.40 - 24.3 %Average value: 14.2 % Grade Count:5
Transmission, Visible 0.000 - 90.0 %Average value: 68.8 % Grade Count:51
 
Processing PropertiesOriginal ValueComments
Processing Temperature 170 - 270 °CAverage value: 212 °C Grade Count:87
Nozzle Temperature 180 - 310 °CAverage value: 238 °C Grade Count:172
Adapter Temperature 200 - 300 °CAverage value: 277 °C Grade Count:31
Die Temperature 200 - 295 °CAverage value: 267 °C Grade Count:31
Melt Temperature 149 - 323 °CAverage value: 234 °C Grade Count:315
Mold Temperature 10.0 - 120 °CAverage value: 62.3 °C Grade Count:377
Injection Velocity 200 - 240 mm/secAverage value: 232 mm/sec Grade Count:30
Roll Temperature 60.0 - 150 °CAverage value: 127 °C Grade Count:29
Drying Temperature 60.0 - 120 °CAverage value: 84.2 °C Grade Count:381
Moisture Content 0.0100 - 0.300 %Average value: 0.0668 % Grade Count:115
Dew Point -29.0 - -17.8 °CAverage value: -19.6 °C Grade Count:6
Injection Pressure 4.14 - 130 MPaAverage value: 56.9 MPa Grade Count:35
Vent Depth 0.00254 - 0.0510 cmAverage value: 0.0123 cm Grade Count:10

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Overview of materials for Acrylonitrile Butadiene Styrene (ABS), Unreinforced, Flame Retardant
Overview of materials for PVC, Molded
Overview of materials for Polypropylene, Molded
Overview of materials for Acrylonitrile Butadiene Styrene (ABS), Extruded
Overview of materials for Acrylonitrile Butadiene Styrene (ABS), Heat Resistant, Molded

O1100 / 77793

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.