MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Copper, UNS C42200, H10 Temper flat products
Categories: Metal; Nonferrous Metal; Copper Alloy

Material Notes: Good to excellent corrosion resistance. Excellent cold workability, good hot formability. Fabricated by blanking, piercing, forming and drawing.

Applications: sash chains, fuse clips, terminals, spring washers, contact springs, electrical connectors.

Test specimen: flat products - 1mm thickness.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 8.80 g/cc0.318 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell B >= 86>= 86
Hardness, Rockwell 30T >= 74>= 74
Tensile Strength, Ultimate >= 605 MPa>= 87700 psi
Tensile Strength, Yield  515 MPa
@Strain 0.5 %
74700 psi
@Strain 0.5 %
 580 MPa
@Strain 0.2 %
84100 psi
@Strain 0.2 %
 580 MPa
@Strain 0.2 %
84100 psi
@Strain 0.2 %
Elongation at Break 2.0 %2.0 %In 50 mm
Modulus of Elasticity 110 GPa16000 ksiHard
 125 GPa18100 ksiAnnealed
Machinability 30 %30 %UNS C36000 (free-cutting brass) = 100%
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000550 ohm-cm
@Temperature 20.0 °C
0.00000550 ohm-cm
@Temperature 68.0 °F
 
Thermal PropertiesMetricEnglishComments
Specific Heat Capacity 0.377 J/g-°C0.0900 BTU/lb-°F
Thermal Conductivity 130 W/m-K
@Temperature 20.0 °C
902 BTU-in/hr-ft²-°F
@Temperature 68.0 °F
Melting Point 1020 - 1040 °C1870 - 1900 °F
Solidus 1020 °C1870 °F
Liquidus 1040 °C1900 °F
Annealing Point 499 - 677 °C930 - 1250 °F
 
Processing PropertiesMetricEnglishComments
Annealing Temperature 500 - 675 °C932 - 1250 °F
Hot-Working Temperature 830 - 890 °C1530 - 1630 °F
 
Component Elements PropertiesMetricEnglishComments
Copper, Cu 89 - 89 %89 - 89 %
Iron, Fe <= 0.050 %<= 0.050 %
Lead, Pb <= 0.050 %<= 0.050 %
Phosphorus, P <= 0.35 %<= 0.35 %
Tin, Sn 0.80 - 1.4 %0.80 - 1.4 %
Zinc, Zn 11.4 %11.4 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

MC42200c2 / 11321

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.