MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Solvay CYCOM® 5250-4 RTM BMI Resin, Unreinforced
Categories: Polymer; Thermoset; Bismaleimide (BMI)

Material Notes: CYCOM® 5250-4 RTM is a true one-part homogeneous BMI resin developed specifically for the resin transfer molding (RTM) process. It reaches very low viscosity during transfer and maintains a low viscosity for several hours, thus providing the maximum capability to fabricate complex parts. Laminates fabricated from CYCOM 5250-4 RTM are capable of service temperatures up to 400°F (204°C), but its toughness and processability make it an ideal material for 180°F (82°C) temperature applications where epoxies are commonly used. CYCOM 5250-4 RTM offers the highest open hole compression (OHC) value of any organic matrix resin while providing the highest level of toughness available in an RTM capable matrix resin.

Features & Benefits:

  • Excellent toughness
  • Maximum continuous service temperature up to 400°F (204°C)
  • Superior hot/wet properties at 160 to 375°F (71 to190°C)
  • Low viscosity during processing
  • Low-tack, solid at room temperature provides ease of handling
  • Low thermal conductivity
  • Versatile cure, can be cured at 400°F (204°C) for 2 hours
  • Out-time greater than 60 days at room temperature
  • True one-part formulation
  • Fully compatible CYCOM 5240-4 RTM low resin content prepregs and CYCOM 782 RTM bindercoated fabrics are available for preform manufacture
Applications:
  • Wing stabilizer spars
  • Fuselage skins and stiffeners
  • Low operating temperature, critical load-bearing components
  • Engine components

Information provided by Cytec, subsequently acquired by Solvay.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.25 g/ccStandard Cure
 1.25 g/ccCure 204°C for 2 hrs no post cure
Water Absorption 3.9 %
@Temperature 71.1 °C,
Time 3.60e+6 sec
Cure 204°C for 2 hrs no post cure
 4.2 %
@Temperature 71.1 °C,
Time 3.60e+6 sec
Standard Cure
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength 14900 psiStandard Cure
 15000 psiCure 204°C for 2 hrs no post cure
Elongation at Break 4.8 %Standard Cure
 4.9 %Cure 204°C for 2 hrs no post cure
Tensile Modulus 4.60 GPaStandard Cure
 4.60 GPaCure 204°C for 2 hrs no post cure
Flexural Strength 23500 psiCure 204°C for 2 hrs no post cure
 23600 psiStandard Cure
Fracture Toughness 0.850 MPa-m½K1C Notch Sensitivity
Charpy Impact Unnotched 97.0 ft-lb/in²Standard Cure
 
Thermal PropertiesOriginal ValueComments
CTE, linear 44.0 µm/m-°CResin after standard cure + postcure
Maximum Service Temperature, Air 204 °Ccontinuous
Glass Transition Temp, Tg 199 °CCure 204°C for 2 hrs-no postcure, wet
 207 °CStandard Cure+Standard Postcure, wet
 254 °CCure 204°C for 2 hrs-no postcure, dry
 271 °CStandard Cure+Standard Postcure, dry
 
Processing PropertiesOriginal ValueComments
Processing Temperature 350 - 375 °F
@Time 21600 sec
Standard Cure. Standard post cure is 440°F for 4 hours
 <= 400 °F
@Time 7200 sec
optional cure (no postcure)
Gel Time 35.0 min
@Temperature 177 °C
Shelf Life 6.00 Month
@Temperature <=-17.8 °C
sealed container

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Solvay CYCOM® 5250-4 BMI Prepreg System with IM-7 Carbon Fiber
Solvay CYCOM® 5250-4 BMI Prepreg Neat Resin
Hexcel® HexPly® F650 Bismaleimide Resin
Solvay CORFIL® 5250-4 Potting Compound
Solvay CYCOM® 5250-4 RTM BMI Resin, Composite with IM7-6K-4HS Fabric

PCYTED079 / 180381

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.