MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

SABIC LNP™ COLORCOMP™ Compound DX06407 Polycarbonate (PC)
Categories: Polymer; Thermoplastic; Polycarbonate (PC)

Material Notes: LNP COLORCOMP DX06407 compound is based on Polycarbonate (PC) resin. Added features of this grade include: Easy Molding, Good Mold Release, Healthcare.

Features: Aesthetics and Appearance,Custom Color,Good Mold Release,Easy Molding

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.20 g/cc1.20 g/ccASTM D792
Density 1.20 g/cc0.0434 lb/in³ASTM D792
Moisture Absorption 0.0200 %0.0200 %Injection Molding
Linear Mold Shrinkage, Flow 0.0070 - 0.0090 cm/cm0.0070 - 0.0090 in/in24hrs; ASTM D955
Linear Mold Shrinkage, Transverse 0.010 - 0.030 cm/cm0.010 - 0.030 in/in24hrs; ASTM D955
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 54.0 MPa7830 psi5 mm/min; ISO 527
 58.0 MPa8410 psi5 mm/min; ASTM D638
Tensile Strength, Yield 63.0 MPa9140 psi5 mm/min; ASTM D638
 65.0 MPa9430 psi5 mm/min; ISO 527
Elongation at Break 94 %94 %5 mm/min; ASTM D638
 104 %104 %5 mm/min; ISO 527
Elongation at Yield 6.2 %6.2 %5 mm/min; ASTM D638
 6.3 %6.3 %5 mm/min; ISO 527
Tensile Modulus 2.30 GPa334 ksi1 mm/min; ISO 527
 2.34 GPa339 ksi5 mm/min; ASTM D638
Flexural Strength 91.0 MPa13200 psiISO 178
Flexural Modulus 2.29 GPa332 ksi2 mm/min; ISO 178
 2.40 GPa348 ksi1.3 mm/min, 50 mm span; ASTM D790
Izod Impact Notched 781 J576 ft-lbASTM D256
Izod Impact, Unnotched 13.1 J/cm24.5 ft-lb/inASTM D4812
Izod Impact, Notched (ISO) 9.00 kJ/m²4.28 ft-lb/in²80*10*4; ISO 180/1A
Izod Impact, Unnotched (ISO) 224 kJ/m²107 ft-lb/in²80*10*4; ISO 180/1U
Dart Drop, Total Energy 63.0 J46.5 ft-lbASTM D3763
Impact Test 69.0 J50.9 ft-lbMultiaxial Impact; ISO 6603
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 0.46 MPa (66 psi) 104 °C219 °FFlatw 80*10*4 sp=64mm; ISO 75/Bf
 103 °C
@Thickness 3.20 mm
217 °F
@Thickness 0.126 in
unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 96.0 °C205 °FFlatw 80*10*4 sp=64mm; ISO 75/Af
 94.0 °C
@Thickness 3.20 mm
201 °F
@Thickness 0.126 in
unannealed; ASTM D648
 
Processing PropertiesMetricEnglishComments
Zone 2 310 - 320 °C590 - 608 °F
Zone 3 320 - 330 °C608 - 626 °F
Melt Temperature 305 - 325 °C581 - 617 °FInjection Molding
Mold Temperature 80.0 - 110 °C176 - 230 °F
Drying Temperature 120 °C248 °FInjection Molding
Dry Time 4.00 hour4.00 hourInjection Molding
Back Pressure 0.200 - 0.300 MPa29.0 - 43.5 psi
Screw Speed 30 - 60 rpm30 - 60 rpm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PSABH80545 / 288492

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.