MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
North American Eastern Cottonwood Wood
Categories: Wood and Natural Products; Wood; Hardwood

Material Notes: Diffuse-Porous Hardwood. Data is based on small, clear, air-dried samples unless specified.

Property values marked by an asterisk (*) have been taken from an unusually old reference source.

Key Words: Populus deltoides; Lumber, Timber
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.370 g/ccOven Dry Weight/Unseasoned Volume
 49.0 lb/ft³Unseasoned*
Cell Length 1.00 mmMature Wood
 
Mechanical PropertiesOriginal ValueComments
Hardness, Wood Indentation 1500 NSide. Force required to imbed a 0.444 inch steel ball to one-half its diameter
 1700 NEnd. Force required to imbed a 0.444 inch steel ball to one-half its diameter
 1900 NSide
Tensile Strength, Ultimate 4.00 MPaPerpendicular to Grain
 410 psiPerpendicular to Grain*
Modulus of Rupture 0.0590 GPaStatic Bending
 5.30 ksiStatic Bending*
Flexural Yield Strength 2900 psiFiber Stress at Elastic Limit; Static Bending*
Flexural Modulus 9.45 GPaStatic Bending
 1010 ksiStatic Bending*
Compressive Strength 3.30 MPaPerpendicular to Grain
 34.0 MPaParallel to Grain
 240 psiPerpendicular to Grain*
 1770 psiParallel to Grain*
 2280 psiMax Crushing Strength Parallel to Grain*
Poissons Ratio 0.018µTL, 12% Moisture Content
 0.043µRL, 12% Moisture Content
 0.292µTR, 12% Moisture Content
 0.344µLR, 12% Moisture Content
 0.42µLT, 12% Moisture Content
 0.875µRT, 12% Moisture Content
Shear Strength 6.40 MPaOrientation Unknown
 680 psiParallel to Grain*
Impact 2.3in-lb/in³; Work to Elastic Limit; Unseasoned Sample; Impact Bending*
 7200psi; Fiber Stress at Elastic Limit; Unseasoned Sample; Impact Bending*
Work to Elastic Limit 0.490 in-lb/in³Static Bending*
Work to Maximum Load 7.30 in-lb/in³Static Bending*
 
Thermal PropertiesOriginal ValueComments
Thermal Conductivity 0.710 BTU-in/hr-ft²-°FOven Dry
 0.850 BTU-in/hr-ft²-°F12% Moisture Content
Shrinkage 3.9 %Radial; Green to Zero Moisture
 9.2 %Tangential; Green to Zero Moisture
 14.1 %Volumetric; Green to Zero Moisture

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
North American Black Willow Wood
North American Engelmann Spruce Wood
North American Elm Wood
American Red Maple Wood
American Chestnut Wood

PTSA100 / 71248

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.