Physical Properties | Metric | English | Comments |
---|
Density | >= 19.3 g/cc | >= 0.697 lb/in³ |
a Lattice Constant | 3.1585 Å | 3.1585 Å |
Vapor Pressure | 2.57311e-018 bar @Temperature 1527 °C | 1.93e-15 torr @Temperature 2781 °F |
| 1.05e-11 bar @Temperature 2127 °C | 7.90e-9 torr @Temperature 3861 °F |
| 5.32e-11 bar @Temperature 2000 °C | 3.99e-8 torr @Temperature 3630 °F |
| 6.67e-9 bar @Temperature 2500 °C | 0.00000500 torr @Temperature 4530 °F |
| 8.67e-8 bar @Temperature 2727 °C | 0.0000650 torr @Temperature 4941 °F |
| 0.00000133 bar @Temperature 3000 °C | 0.000997 torr @Temperature 5430 °F |
| 0.00000624 bar @Temperature 3227 °C | 0.00468 torr @Temperature 5841 °F |
|
Chemical Properties | Metric | English | Comments |
---|
Atomic Mass | 183.92 | 183.92 |
Atomic Number | 74 | 74 |
Atomic Volume | 9.53 | 9.53 |
|
Mechanical Properties | Metric | English | Comments |
---|
Modulus of Elasticity | 407 GPa | 59000 ksi |
|
Electrical Properties | Metric | English | Comments |
---|
Electrical Resistivity | 0.00000550 ohm-cm @Temperature 20.0 °C | 0.00000550 ohm-cm @Temperature 68.0 °F |
| 0.00000728 ohm-cm @Temperature 100 °C | 0.00000728 ohm-cm @Temperature 212 °F |
| 0.0000180 ohm-cm @Temperature 500 °C | 0.0000180 ohm-cm @Temperature 932 °F |
| 0.00002243 ohm-cm @Temperature 700 °C | 0.00002243 ohm-cm @Temperature 1290 °F |
| 0.0000330 ohm-cm @Temperature 1000 °C | 0.0000330 ohm-cm @Temperature 1830 °F |
| 0.00003465 ohm-cm @Temperature 1100 °C | 0.00003465 ohm-cm @Temperature 2010 °F |
| 0.00004966 ohm-cm @Temperature 1500 °C | 0.00004966 ohm-cm @Temperature 2730 °F |
| 0.00005752 ohm-cm @Temperature 1800 °C | 0.00005752 ohm-cm @Temperature 3270 °F |
| 0.00006961 ohm-cm @Temperature 2100 °C | 0.00006961 ohm-cm @Temperature 3810 °F |
| 0.00100 ohm-cm @Temperature 3000 °C | 0.00100 ohm-cm @Temperature 5430 °F |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear | 4.45 µm/m-°C @Temperature 0.000 - 500 °C | 2.47 µin/in-°F @Temperature 32.0 - 932 °F |
| 4.98 µm/m-°C @Temperature 0.000 - 500 °C | 2.77 µin/in-°F @Temperature 32.0 - 932 °F |
Specific Heat Capacity | 0.140 J/g-°C | 0.0335 BTU/lb-°F |
Thermal Conductivity | 92.9 W/m-K @Temperature 2000 °C | 644 BTU-in/hr-ft²-°F @Temperature 3630 °F |
| 103 W/m-K @Temperature 1727 °C | 710 BTU-in/hr-ft²-°F @Temperature 3141 °F |
| 106 W/m-K @Temperature 1527 °C | 733 BTU-in/hr-ft²-°F @Temperature 2781 °F |
| 109 W/m-K @Temperature 1327 °C | 754 BTU-in/hr-ft²-°F @Temperature 2421 °F |
| 112 W/m-K @Temperature 1127 °C | 777 BTU-in/hr-ft²-°F @Temperature 2061 °F |
| 115 W/m-K @Temperature 927 °C | 797 BTU-in/hr-ft²-°F @Temperature 1700 °F |
| 121 W/m-K @Temperature 500 °C | 841 BTU-in/hr-ft²-°F @Temperature 932 °F |
| 159 W/m-K @Temperature 100 °C | 1100 BTU-in/hr-ft²-°F @Temperature 212 °F |
| 167 W/m-K @Temperature 20.0 °C | 1160 BTU-in/hr-ft²-°F @Temperature 68.0 °F |
Melting Point | 3410 °C | 6170 °F |
Boiling Point | 5900 °C | 10700 °F |
|
Component Elements Properties | Metric | English | Comments |
---|
Aluminum, Al | <= 0.0025 % | <= 0.0025 % |
Carbon, C | <= 0.0050 % | <= 0.0050 % |
Chromium, Cr | <= 0.0020 % | <= 0.0020 % |
Copper, Cu | <= 0.0010 % | <= 0.0010 % |
Iron, Fe | <= 0.0030 % | <= 0.0030 % |
Molybdenum, Mo | <= 0.0050 % | <= 0.0050 % |
Nickel, Ni | <= 0.0030 % | <= 0.0030 % |
Other, each | <= 0.0020 % | <= 0.0020 % |
Oxygen, O | <= 0.0050 % | <= 0.0050 % |
Potassium, K | <= 0.0020 % | <= 0.0020 % |
Silicon, Si | <= 0.0040 % | <= 0.0040 % |
Sodium, Na | <= 0.0020 % | <= 0.0020 % |
Tungsten, W | >= 99.95 % | >= 99.95 % |
|
Descriptive Properties |
---|
Electron Work Function | 4.55 |
Lattice Structure | Body Centered Cubic |
RoHS Compliance | 2002/95/EC |
Some of the values displayed above may have been converted from their original units and/or rounded in order to
display the information in a consistent format. Users requiring more precise data for scientific or engineering
calculations can click on the property value to see the original value as well as raw conversions to equivalent units.
We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding
error. We also ask that you refer to MatWeb's
terms of use regarding this information.
Click here to view
all the property values for this datasheet as they were originally entered into MatWeb.