Physical Properties | Original Value | Comments |
---|
Density | 1.315 - 1.325 g/cc |
| 1.124 g/cc @Temperature 210 °C |
| 1.137 g/cc @Temperature 200 °C |
| 1.146 g/cc @Temperature 190 °C |
| 1.161 g/cc @Temperature 180 °C |
| 1.173 g/cc @Temperature 170 °C |
| 1.184 g/cc @Temperature 160 °C |
| 1.195 g/cc @Temperature 150 °C |
| 1.206 g/cc @Temperature 140 °C |
| 1.216 g/cc @Temperature 130 °C |
| 1.227 g/cc @Temperature 120 °C |
| 1.237 g/cc @Temperature 110 °C |
| 1.247 g/cc @Temperature 100 °C |
| 1.257 g/cc @Temperature 90.0 °C |
| 1.266 g/cc @Temperature 80.0 °C |
| 1.276 g/cc @Temperature 70.0 °C |
| 1.284 g/cc @Temperature 60.0 °C |
| 1.294 g/cc @Temperature 50.0 °C |
| 1.303 g/cc @Temperature 40.0 °C |
| 1.312 g/cc @Temperature 30.0 °C |
| 1.321 g/cc @Temperature 20.0 °C |
| 1.329 g/cc @Temperature 10.0 °C |
| 1.338 g/cc @Temperature 0.000 °C |
Viscosity | 0.23 cP @Temperature 210 °C |
| 0.35 cP @Temperature 200 °C |
| 0.51 cP @Temperature 190 °C |
| 0.69 cP @Temperature 180 °C |
| 0.91 cP @Temperature 170 °C |
| 1.15 cP @Temperature 160 °C |
| 1.43 cP @Temperature 150 °C |
| 1.76 cP @Temperature 140 °C |
| 2.15 cP @Temperature 130 °C |
| 2.65 cP @Temperature 120 °C |
| 3.31 cP @Temperature 110 °C |
| 4.23 cP @Temperature 100 °C |
| 5.6 cP @Temperature 90.0 °C |
| 7.72 cP @Temperature 80.0 °C |
| 11.2 cP @Temperature 70.0 °C |
| 17.3 cP @Temperature 60.0 °C |
| 28.6 cP @Temperature 50.0 °C |
| 51.2 cP @Temperature 40.0 °C |
| 100 cP @Temperature 30.0 °C |
| 215 cP @Temperature 20.0 °C |
| 516 cP @Temperature 10.0 °C |
Molecular Weight | 110.54 g/mol |
Vapor Pressure | <= 0.00000987 atm @Temperature 0.000 °C |
| <= 0.00000987 atm @Temperature 10.0 °C |
| <= 0.00000987 atm @Temperature 20.0 °C |
| 0.00000987 atm @Temperature 30.0 °C |
| 0.0000296 atm @Temperature 40.0 °C |
| 0.0000789 atm @Temperature 50.0 °C |
| 0.000227 atm @Temperature 60.0 °C |
| 0.000570 atm @Temperature 70.0 °C |
| 0.00131 atm @Temperature 80.0 °C |
| 0.00280 atm @Temperature 90.0 °C |
| 0.00570 atm @Temperature 100 °C |
| 0.0110 atm @Temperature 110 °C |
| 0.0130 atm @Temperature 115 °C |
| 0.0198 atm @Temperature 120 °C |
| 0.0345 atm @Temperature 130 °C |
| 0.0581 atm @Temperature 140 °C |
| 0.0942 atm @Temperature 150 °C |
| 0.148 atm @Temperature 160 °C |
| 0.226 atm @Temperature 170 °C |
| 0.337 atm @Temperature 180 °C |
| 0.490 atm @Temperature 190 °C |
| 0.698 atm @Temperature 200 °C |
| 0.975 atm @Temperature 210 °C |
|
Chemical Properties | Original Value | Comments |
---|
Critical Pressure | 53.7 bar |
Critical Temperature | 430 °C |
|
Thermal Properties | Original Value | Comments |
---|
Heat of Vaporization | 475 J/g |
Melting Point | -40.0 °C |
Boiling Point | 115 °C @Pressure 0.0133 MPa |
| 198 - 213 °C @Pressure 1.013 MPa |
Decomposition Temperature | >= 213 °C |
Flash Point | 145 °C |
|
Descriptive Properties |
---|
Appearance | Clear without suspended matter |
Color | <40 |
Composition | <0.35 g/kg |
| <1 g/kg |
| <1.5 g/kg |
| >98.5 g/kg |
Some of the values displayed above may have been converted from their original units and/or rounded in order to
display the information in a consistent format. Users requiring more precise data for scientific or engineering
calculations can click on the property value to see the original value as well as raw conversions to equivalent units.
We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding
error. We also ask that you refer to MatWeb's
terms of use regarding this information.
Click here to go back to viewing the property data in MatWeb's normal format.