MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Teknor Apex Sarlink® TPV X17180B Thermoplastic Vulcanizate
Categories: Polymer; Thermoplastic; Elastomer, TPE; Thermoplastic Vulcanizate Elastomer (TPV)

Material Notes: Notes: Sarlink TPV 17100 series is the latest generation of super high-flow TPV materials ensuring the best in class surface appearance of injection parts. This product is a medium hardness, low density, high performance thermoplastic vulcanizate that exhibits excellent UV resistance elasticity, and surface aesthetics designed for demanding automotive applications including window encapsulation and exterior parts.

Availability: Africa & Middle East; Asia Pacific; Europe; Latin America; North America

Features: Chemical Resistant; Good Adhesion; Good Flexibility; Good Moldability; Good Surface Finish; High Elasticity; High Flow; High Heat Resistance; Low Compression Set; Low Density; Low Specific Gravity; Medium Hardness; UV Resistant

Uses: Automotive Applications; Automotive Exterior Parts; Automotive Window Encapsulation; Rubber Replacement

RoHS Compliance: RoHS Compliant

Form: Pellets

Processing Method: Injection Molding

Preliminary data. Information provided by Teknor Apex

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.915 g/cc0.0331 lb/in³ISO 1183
Viscosity 188 cP
@Shear Rate 206 1/s,
Temperature 200 °C
188 cP
@Shear Rate 206 1/s,
Temperature 392 °F
Apparent; ASTM D3835
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A  80
@Time 5.00 sec
80
@Time 0.00139 hour
Injection Molded; ISO 868
 82
@Time 5.00 sec
82
@Time 0.00139 hour
Extruded; ISO 868
Tensile Strength at Break 5.40 MPa783 psiAcross Flow; ISO 37
 5.50 MPa798 psiFlow; ISO 37
 4.64 MPa
@Treatment Temp. 150 °C,
Time 605000 sec
673 psi
@Treatment Temp. 302 °F,
Time 168 hour
Across Flow, Change in Air; ISO 37
Tensile Stress at Strain  3.13 MPa
@Strain 100 %
454 psi
@Strain 100 %
Across Flow; ISO 37
 3.50 MPa
@Strain 100 %
508 psi
@Strain 100 %
Flow; ISO 37
Elongation at Break 400 %400 %Flow; ISO 37
 460 %460 %Across Flow; ISO 37
 336 %
@Treatment Temp. 150 °C,
Time 605000 sec
336 %
@Treatment Temp. 302 °F,
Time 168 hour
Across Flow, Change in Air; ISO 37
Tear Strength 26.3 kN/m150 pliMethod Ba, Angle (Unnicked), Flow; ISO 34-1
 28.0 kN/m160 pliMethod Ba, Angle (Unnicked), Across Flow; ISO 34-1
Compression Set  31 %
@Temperature 22.8 °C,
Time 79200 sec
31 %
@Temperature 73.0 °F,
Time 22.0 hour
ISO 815
 43 %
@Temperature 70.0 °C,
Time 79200 sec
43 %
@Temperature 158 °F,
Time 22.0 hour
ISO 815
 64 %
@Temperature 125 °C,
Time 252000 sec
64 %
@Temperature 257 °F,
Time 70.0 hour
ISO 815
 
Processing PropertiesMetricEnglishComments
Rear Barrel Temperature 180 - 205 °C356 - 401 °F
Middle Barrel Temperature 180 - 205 °C356 - 401 °F
Front Barrel Temperature 180 - 205 °C356 - 401 °F
Nozzle Temperature 185 - 210 °C365 - 410 °F
Melt Temperature 185 - 210 °C365 - 410 °F
Mold Temperature 10.0 - 55.0 °C50.0 - 131 °F
Drying Temperature 82.2 °C180 °F
Dry Time 3.00 hour3.00 hour
Back Pressure 0.100 - 1.00 MPa14.5 - 145 psi
Screw Speed 100 - 200 rpm100 - 200 rpm
 
Descriptive Properties
AppearanceBlack

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PTEKNQ1230 / 237721

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.