MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

SABIC LNP™ STAT-KON™ Compound DX04489C Polycarbonate (PC)
Categories: Polymer; Thermoplastic; Polycarbonate (PC)

Material Notes: LNP STAT-KON DX04489C compound is based on Polycarbonate (PC) resin containing 30% carbon fiber. Added features of this grade include: LNP Clean Compounding Technology, High Modulus, Electrically Conductive.

Features: LNP Clean Compound Technology,High Stiffness,Light-weight Structural,Super Strong (Carbon Fiber Filled),Electrically Conductive

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.33 g/cc0.0480 lb/in³ASTM D792
Moisture Absorption 0.0200 %0.0200 %Injection Molding
 0.100 %0.100 %23°C/50% RH/24 hrs; ASTM D570
Linear Mold Shrinkage, Transverse 0.0030 cm/cm0.0030 in/in24hrs; ASTM D955
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 111 MPa16100 psiASTM D638
Tensile Strength, Yield 130 MPa18900 psiASTM D638
Elongation at Break 2.4 %2.4 %ASTM D638
Elongation at Yield 2.2 %2.2 %ASTM D638
Tensile Modulus 16.63 GPa2412 ksi50 mm/min; ASTM D638
Flexural Strength 206 MPa29900 psiASTM D790
Flexural Modulus 15.53 GPa2252 ksiASTM D790
Izod Impact Notched 58.0 J42.8 ft-lbASTM D256
Izod Impact, Unnotched 4.80 J/cm8.99 ft-lb/inASTM D4812
Dart Drop, Total Energy 11.0 J8.11 ft-lbpeak; ASTM D3763
 
Electrical PropertiesMetricEnglishComments
Surface Resistance 100 - 1.00e+6 ohm100 - 1.00e+6 ohmASTM D257
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 16.2 µm/m-°C
@Temperature -40.0 - 40.0 °C
9.00 µin/in-°F
@Temperature -40.0 - 104 °F
ASTM E831
CTE, linear, Transverse to Flow 41.4 µm/m-°C
@Temperature -40.0 - 40.0 °C
23.0 µin/in-°F
@Temperature -40.0 - 104 °F
ASTM E831
Deflection Temperature at 1.8 MPa (264 psi) 140 °C
@Thickness 3.20 mm
284 °F
@Thickness 0.126 in
unannealed; ASTM D648
UL RTI, Electrical 80.0 °C176 °FUL 746B
UL RTI, Mechanical with Impact 80.0 °C176 °FUL 746B
UL RTI, Mechanical without Impact 80.0 °C176 °FUL 746B
Flammability, UL94 V-2
@Thickness 1.50 mm
V-2
@Thickness 0.0591 in
UL 94
 
Processing PropertiesMetricEnglishComments
Zone 2 310 - 320 °C590 - 608 °F
Zone 3 320 - 330 °C608 - 626 °F
Melt Temperature 305 - 325 °C581 - 617 °FInjection Molding
Mold Temperature 80.0 - 110 °C176 - 230 °F
Drying Temperature 120 °C248 °FInjection Molding
Dry Time 4.00 hour4.00 hourInjection Molding
Back Pressure 0.200 - 0.300 MPa29.0 - 43.5 psi
Screw Speed 30 - 60 rpm30 - 60 rpm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PSABH81251 / 289198

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.