MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Teknor Apex Sarlink® TPV 4145 Thermoplastic Vulcanizate
Categories: Polymer; Thermoplastic; Elastomer, TPE; Thermoplastic Vulcanizate Elastomer (TPV)

Material Notes: Notes: Sarlink TPV 4100 series are engineered materials designed primarily for demanding automotive and industrial applications. This product is a low density, medium hardness thermoplastic vulcanizate that exhibits excellent compression set, flex fatigue, high and low temperature performance. The material can be processed by injection molding, blow molding and extrusion for applications such as seals, gaskets, chemical resistant hose and tube, boots and bellows.

Availability: Asia Pacific; Europe; Latin America; North America

Features: Chemical Resistant; Excellent Elastic Recovery; Fatigue Resistant; Good Adhesion; Good Flexibility; Good Moldability; Good Processability; Good Surface Finish; High Melt Stability; Low Compression Set; Low Density; Low Hardness; Low Specific Gravity; Medium Heat Resistant; Resilient

Uses: Appliance Components; Automotive Applications; Automotive Exterior Parts; Automotive Interior Parts; Automotive Under the Hood; Blow Molding Applications; Constant Velocity Joint Boots; Flexible Grips; Gaskets; Grommets; Hose; Industrial Applications; O-ring; Pipe Seals; Profiles; Rubber Replacement; Seals; White Goods & Small Appliance

RoHS Compliance: RoHS Compliant

Form: Pellets

Processing Method: Extrusion; Injection Molding; Blow Molding; Profile Extrusion

Information provided by Teknor Apex

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.960 g/cc0.0347 lb/in³ISO 1183
Viscosity 320 cP
@Shear Rate 206 1/s,
Temperature 200 °C
320 cP
@Shear Rate 206 1/s,
Temperature 392 °F
Shear, Capillary; ASTM D3835
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A  45
@Time 5.00 sec
45
@Time 0.00139 hour
Extruded; ISO 868
 48
@Time 5.00 sec
48
@Time 0.00139 hour
Injection Molded; ISO 868
Tensile Strength at Break 3.10 MPa450 psiFlow; ISO 37
 4.30 MPa624 psiAcross Flow; ISO 37
 4.09 MPa
@Treatment Temp. 150 °C,
Time 605000 sec
593 psi
@Treatment Temp. 302 °F,
Time 168 hour
Across Flow, Change in Air; ISO 188
 4.22 MPa
@Treatment Temp. 135 °C,
Time 3.60e+6 sec
612 psi
@Treatment Temp. 275 °F,
Time 1000 hour
Across Flow, Change in Air; ISO 188
Tensile Stress at Strain  1.30 MPa
@Strain 100 %
189 psi
@Strain 100 %
Across Flow; ISO 37
 2.60 MPa
@Strain 100 %
377 psi
@Strain 100 %
Flow; ISO 37
 1.26 MPa
@Strain 100 %,
Treatment Temp. 150 °C
183 psi
@Strain 100 %,
Treatment Temp. 302 °F
Across Flow, Change in Air at 168 hr; ISO 188
 1.30 MPa
@Strain 100 %,
Treatment Temp. 135 °C
189 psi
@Strain 100 %,
Treatment Temp. 275 °F
Across Flow, Change in Air at 1000 hr; ISO 188
Elongation at Break 180 %180 %Flow; ISO 37
 550 %550 %Across Flow; ISO 37
 583 %
@Treatment Temp. 150 °C,
Time 605000 sec
583 %
@Treatment Temp. 302 °F,
Time 168 hour
Across Flow, Change in Air; ISO 188
 622 %
@Treatment Temp. 135 °C,
Time 3.60e+6 sec
622 %
@Treatment Temp. 275 °F,
Time 1000 hour
Across Flow, Change in Air; ISO 188
Tear Strength 19.3 kN/m110 pliMethod Ba, Angle (Unnicked); ISO 34-1
Compression Set  11 %
@Temperature 22.8 °C,
Time 79200 sec
11 %
@Temperature 73.0 °F,
Time 22.0 hour
ISO 815
 26 %
@Temperature 70.0 °C,
Time 79200 sec
26 %
@Temperature 158 °F,
Time 22.0 hour
ISO 815
 35 %
@Temperature 125 °C,
Time 252000 sec
35 %
@Temperature 257 °F,
Time 70.0 hour
ISO 815
 
Thermal PropertiesMetricEnglishComments
UL RTI, Electrical 50.0 °C122 °FUL 746
UL RTI, Mechanical with Impact 50.0 °C122 °FUL 746
UL RTI, Mechanical without Impact 50.0 °C122 °FUL 746
 
Processing PropertiesMetricEnglishComments
Processing Temperature 182 - 221 °C360 - 430 °FInjection
Rear Barrel Temperature 177 - 216 °C350 - 420 °FInjection
Middle Barrel Temperature 177 - 216 °C350 - 420 °FInjection
Front Barrel Temperature 177 - 216 °C350 - 420 °FInjection
Nozzle Temperature 188 - 221 °C370 - 430 °FInjection
Zone 1 182 - 204 °C360 - 400 °FExtrusion
Zone 2 182 - 204 °C360 - 400 °FExtrusion
Zone 3 188 - 210 °C370 - 410 °FExtrusion
Zone 4 188 - 210 °C370 - 410 °FExtrusion
Die Temperature 193 - 216 °C380 - 420 °FExtrusion
Melt Temperature 193 - 216 °C380 - 420 °FExtrusion
Mold Temperature 10.0 - 65.6 °C50.0 - 150 °FInjection
Drying Temperature 82.2 °C180 °F
Dry Time 3.00 hour3.00 hour
Screw Speed 100 - 200 rpm100 - 200 rpmInjection
 
Descriptive Properties
AppearanceBlack
 Natural Color
 Opaque

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PTEKNQ1154 / 237645

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.